General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 0.18 g/cm³ Show Supplier Material materials with Densidad of 0.18 g/cm³ |
Porosidad | 90 % Show Supplier Material materials with Porosidad of 90 % |
Mecánica
Property | Temperature | Value |
---|---|---|
Resistencia a la compresión | 23.0 °C | 0.3 MPa Show Supplier Material materials with Resistencia a la compresión of 0.3 MPa |
Resistencia a la compresión transversal | 23.0 °C | 1 MPa Show Supplier Material materials with Resistencia a la compresión transversal of 1 MPa |
Resistencia a la flexión | 23.0 °C | 1.1 MPa Show Supplier Material materials with Resistencia a la flexión of 1.1 MPa |
Resistencia a la flexión transversal | 23.0 °C | 0.2 MPa Show Supplier Material materials with Resistencia a la flexión transversal of 0.2 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 3.3E-6 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 3.3E-6 1/K | average for 20-100°C |
Coeficiente de dilatación térmica transversal | 23.0 °C | 3E-6 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 3E-6 1/K | average for 20-100°C |
Contenido de cenizas | 23.0 °C | 0.15 % Show Supplier Material materials with Contenido de cenizas of 0.15 % | |
Thermal conductivity, in-plane | 20.0 °C | 0.39 W/(m·K) Show Supplier Material materials with Thermal conductivity, in-plane of 0.39 W/(m·K) | |
1500.0 °C | 1.5 W/(m·K) Show Supplier Material materials with Thermal conductivity, in-plane of 1.5 W/(m·K) | ||
Thermal conductivity, through-plane | 20.0 °C | 0.18 W/(m·K) Show Supplier Material materials with Thermal conductivity, through-plane of 0.18 W/(m·K) | |
1500.0 °C | 0.45 W/(m·K) Show Supplier Material materials with Thermal conductivity, through-plane of 0.45 W/(m·K) | ||
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 23.0 °C | 6.7E-4 Ω·m Show Supplier Material materials with Resistividad eléctrica of 6.7E-4 Ω·m |
Resistividad eléctrica transversal | 23.0 °C | 4.7E-3 Ω·m Show Supplier Material materials with Resistividad eléctrica transversal of 4.7E-3 Ω·m |
Chemical properties
Property | Value |
---|---|
Carbono | 99.9 % Show Supplier Material materials with Carbono of 99.9 % |
Technological properties
Property | ||
---|---|---|
Application areas | Vacuum furnace insulation, Inert atmosphere furnace insulation, Inert atmosphere process equipment insulation, Semiconductor crystal growing furnace insulation | |
Processing history | Hard felt |