Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] | Typical for Cast Copper Bronze |
Módulo elástico | 23.0 °C | 96 - 120 GPa Show Material materials with Módulo elástico of 96 - 120 GPa | Typical for Cast Copper Bronze |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 376 - 440 J/(kg·K) Show Material materials with Calor específico of 376 - 440 J/(kg·K) | Typical for Cast Copper Bronze |
Coeficiente de dilatación térmica | 23.0 °C | 1.6E-5 - 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.9E-5 1/K | Typical for Cast Copper Bronze |
Conductividad térmica | 23.0 °C | 12 - 81 W/(m·K) Show Material materials with Conductividad térmica of 12 - 81 W/(m·K) | Typical for Cast Copper Bronze |
Temperatura de fusión | 760 - 1060 °C Show Material materials with Temperatura de fusión of 760 - 1060 °C | Typical for Cast Copper Bronze |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.01 % Show Material materials with Aluminio of 0.01 % |
Antimonio | 0.2 - 0.3 % Show Material materials with Antimonio of 0.2 - 0.3 % |
Arsénico | 0.1 % Show Material materials with Arsénico of 0.1 % |
Azufre | 0.06 - 0.1 % Show Material materials with Azufre of 0.06 - 0.1 % |
Cobre | 83.5 - 87.5 % Show Material materials with Cobre of 83.5 - 87.5 % |
Estaño | 5.5 - 7 % Show Material materials with Estaño of 5.5 - 7 % |
Fósforo | 0.03 - 0.05 % Show Material materials with Fósforo of 0.03 - 0.05 % |
Hierro | 0.2 - 0.25 % Show Material materials with Hierro of 0.2 - 0.25 % |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % |
Níquel | 1.5 - 2.5 % Show Material materials with Níquel of 1.5 - 2.5 % |
Otro | total 0.5,total 0.4 |
Plomo | 2.5 - 4 % Show Material materials with Plomo of 2.5 - 4 % |
Silicona | 0.01 % Show Material materials with Silicona of 0.01 % |
Zinc | 1.5 - 3 % Show Material materials with Zinc of 1.5 - 3 % |