General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8.8 g/cm³ Show Material materials with Densidad of 8.8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Leaded Phosphor Bronze |
Dureza Brinell | 23.0 °C | 150 [-] Show Material materials with Dureza Brinell of 150 [-] | |
Dureza Vickers | 23.0 °C | 150 [-] Show Material materials with Dureza Vickers of 150 [-] | |
Elongación | 23.0 °C | 10 % Show Material materials with Elongación of 10 % | |
Elongation A100 | 23.0 °C | 6 % Show Material materials with Elongation A100 of 6 % | |
Límite elástico Rp 0,2 | 23.0 °C | 350 MPa Show Material materials with Límite elástico Rp 0,2 of 350 MPa | |
Módulo elástico | 23.0 °C | 110 - 130 GPa Show Material materials with Módulo elástico of 110 - 130 GPa | Typical for Leaded Phosphor Bronze |
Resistencia a la tracción | 23.0 °C | 450 MPa Show Material materials with Resistencia a la tracción of 450 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 380 J/(kg·K) Show Material materials with Calor específico of 380 J/(kg·K) | Typical for Leaded Phosphor Bronze |
Coeficiente de dilatación térmica | 23.0 °C | 1.5E-5 - 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.5E-5 - 1.9E-5 1/K | Typical for Leaded Phosphor Bronze |
Temperatura de fusión | 930 - 1060 °C Show Material materials with Temperatura de fusión of 930 - 1060 °C |
Chemical properties
Property | Value |
---|---|
Estaño | 3.5 - 5.5 % Show Material materials with Estaño of 3.5 - 5.5 % |
Fósforo | 0.01 - 0.4 % Show Material materials with Fósforo of 0.01 - 0.4 % |
Hierro | 0.1 % Show Material materials with Hierro of 0.1 % |
Níquel | 0.2 % Show Material materials with Níquel of 0.2 % |
Otro | Rest Cu, total 0.2 |
Plomo | 0.5 - 1.5 % Show Material materials with Plomo of 0.5 - 1.5 % |
Zinc | 0.3 % Show Material materials with Zinc of 0.3 % |
Technological properties
Property | ||
---|---|---|
Brazing | hard brazing : good to medium, soft brazing: very good to good | |
Workability | Cold forming degree between anneals: max. 75 %, general (condition): good to medium |