General
Property | Value | Testing Standard | Condition |
---|---|---|---|
Absorción de agua | 0.03 % Show Supplier Material materials with Absorción de agua of 0.03 % | Sim. to ISO 62 | |
Densidad | 1.79 g/cm³ Show Supplier Material materials with Densidad of 1.79 g/cm³ | ISO 1183 | dry |
Índice límite de óxigeno | 44 % Show Supplier Material materials with Índice límite de óxigeno of 44 % | ISO 4589-1/-2 | dry |
Mecánica
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Elongación | 50 % Show Supplier Material materials with Elongación of 50 % | dry | ISO 527-1/-2 | min. | nominal |
Elongation at yield | 18 % Show Supplier Material materials with Elongation at yield of 18 % | dry | ISO 527-1/-2 | |
Límite elástico | 10 MPa Show Supplier Material materials with Límite elástico of 10 MPa | dry | ISO 527-1/-2 | |
Módulo elástico | 0.35 GPa Show Supplier Material materials with Módulo elástico of 0.35 GPa | dry | ISO 527-1/-2 |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment | ||||
---|---|---|---|---|---|---|---|---|---|
Temperatura de flexión bajo carga | 31 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 31 °C | dry | ISO 75-1/-2 | 2 MPa | |||||
Temperatura de fusión | 122 °C Show Supplier Material materials with Temperatura de fusión of 122 °C | dry | ISO 11357-1/-3 | 10°C/min | |||||
Temperatura de transición del vidrio | -40 °C Show Supplier Material materials with Temperatura de transición del vidrio of -40 °C | dry | ISO 11357-1/-2 | 10°C/min | |||||
Inflamabilidad | At thickness 1.5 mm IEC 60695-11-10: V-0, At thickness 1 mm IEC 60695-11-10: V-0 and yellow card available |
Eléctrico
Property | Value | Condition | Testing Standard |
---|---|---|---|
Rigidez dieléctrica | 12 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 12 kV/mm | dry | IEC 60243-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Velocidad de flujo del volumen derretido | 5.8 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 5.8 cm³/10min | dry | ISO 1133 | 232°C/3.8kg |
Technological properties
Property | ||
---|---|---|
Application areas | Fluoropolymer Processing Aids | |
Certifications | Yellow Card |