Material: el 'Kovar® Plate' que buscabas ha sido remplazado por el material siguiente.

Kovar® Plate

View suppliers (15)
Nombres alternativos y comerciales
Pernifer 2918®, Dilvar P1®, NILO K®
Want to keep this datasheet? Save it now in your required format

Description

Kovar is a controlled expansion alloy. It is a nickel iron alloy with 29% nickel, 17% cobalt and the remaining balance is iron. The expansion characteristics of Kovar match both borosilicate (or Pyrex) glasses and alumina ceramics, making it one of the most popular of the controlled expansion alloys for hermetic sealing applications. Kovar is produced to ensure good properties for machining and deep drawing, and is a porosity free product.

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por Matmatch.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValue

Densidad

23.0 °C

8.36 g/cm³

Show Material materials with Densidad of 8.36 g/cm³

Medidas

PropertyValue

Ancho

381 mm

Show Material materials with Ancho of 381 mm

Espesor

4.8 - 31.8 mm

Show Material materials with Espesor of 4.8 - 31.8 mm

Longitud

1828 mm

Show Material materials with Longitud of 1828 mm

Dimensions

Available thicknesses: 4.8mm, 6.4mm, 7.1mm, 7.9mm, 9.5mm, 11.1mm, 12.7mm, 15.9mm, 19.1mm, 25.4mm, 31.8mm

Mecánica

PropertyTemperatureValueComment

Dureza Rockwell B

23.0 °C

80 [-]

Show Material materials with Dureza Rockwell B of 80 [-]

Elongación

23.0 °C

30 %

Show Material materials with Elongación of 30 %

in 2 in.

Límite elástico

23.0 °C

276 MPa

Show Material materials with Límite elástico of 276 MPa

Módulo elástico

23.0 °C

207 GPa

Show Material materials with Módulo elástico of 207 GPa

Resistencia a la tracción

23.0 °C

518 MPa

Show Material materials with Resistencia a la tracción of 518 MPa

Aplicaciones térmicas

PropertyTemperatureValueComment

Calor específico

23.0 °C

460 J/(kg·K)

Show Material materials with Calor específico of 460 J/(kg·K)

Coeficiente de dilatación térmica

100.0 °C

5.8E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 5.8E-6 1/K

from 30°C to the mentioned temperature

150.0 °C

5.6E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 5.6E-6 1/K

from 30°C to the mentioned temperature

200.0 °C

5.4E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 5.4E-6 1/K

from 30°C to the mentioned temperature

250.0 °C

5.3E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 5.3E-6 1/K

from 30°C to the mentioned temperature

300.0 °C

5.1E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 5.1E-6 1/K

from 30°C to the mentioned temperature

350.0 °C

4.9E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 4.9E-6 1/K

from 30°C to the mentioned temperature

400.0 °C

4.6E-6 - 5.2E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 4.6E-6 - 5.2E-6 1/K

from 30°C to the mentioned temperature

450.0 °C

5.1E-6 - 5.5E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 5.1E-6 - 5.5E-6 1/K

from 30°C to the mentioned temperature

500.0 °C

6.1E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 6.1E-6 1/K

from 30°C to the mentioned temperature

550.0 °C

6.8E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 6.8E-6 1/K

from 30°C to the mentioned temperature

600.0 °C

7.5E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 7.5E-6 1/K

from 30°C to the mentioned temperature

700.0 °C

8.7E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 8.7E-6 1/K

from 30°C to the mentioned temperature

800.0 °C

1.03E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.03E-5 1/K

from 30°C to the mentioned temperature

900.0 °C

1.08E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K

from 30°C to the mentioned temperature

1039.0 °C

1.17E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.17E-5 1/K

from 30°C to the mentioned temperature

Conductividad térmica

23.0 °C

17 W/(m·K)

Show Material materials with Conductividad térmica of 17 W/(m·K)

Temperatura de fusión

1449 °C

Show Material materials with Temperatura de fusión of 1449 °C

Eléctrico

PropertyTemperatureValue

Resistividad eléctrica

23.0 °C

4E-7 Ω·m

Show Material materials with Resistividad eléctrica of 4E-7 Ω·m

Magnético

PropertyValue

Temperatura de Curie

435 °C

Show Material materials with Temperatura de Curie of 435 °C

Chemical properties

PropertyValue

Carbono

0.02 %

Show Material materials with Carbono of 0.02 %

Cobalto

17 %

Show Material materials with Cobalto of 17 %

Cromo

0.2 %

Show Material materials with Cromo of 0.2 %

Hierro

Balance

Níquel

29 %

Show Material materials with Níquel of 29 %

Silicona

0.2 %

Show Material materials with Silicona of 0.2 %

Technological properties

Property
Application areas

Common applications of Kovar: Glass-to-metal hermetic sealing with hard borosilicate glass, ceramic-to-metal sealing, power tubes, microwave tubes, transistors, diodes, integrated circuits, hybrid packages

Looking for suppliers of this material? Click to see 15 supplier of Kovar® Plate on Matmatch