General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 1.17 g/cm³ Show Material materials with Densidad of 1.17 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 11 % Show Material materials with Elongación of 11 % | ASTM D 638 | Type I, 5 mm/min |
Elongation at yield | 23.0 °C | 2.1 % Show Material materials with Elongation at yield of 2.1 % | ASTM D 638 | Type I, 5 mm/min |
Flexural yield strength | 23.0 °C | 73 MPa Show Material materials with Flexural yield strength of 73 MPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Impact strength, Izod notched, ASTM | 23.0 °C | 267 J/m Show Material materials with Impact strength, Izod notched, ASTM of 267 J/m | ASTM D 256 |
Límite elástico | 23.0 °C | 42 MPa Show Material materials with Límite elástico of 42 MPa | ASTM D 638 | Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 2.72 GPa Show Material materials with Módulo de flexión of 2.72 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Módulo elástico | 23.0 °C | 2.41 GPa Show Material materials with Módulo elástico of 2.41 GPa | ASTM D 638 | 5 mm/min |
Resistencia a la tracción | 23.0 °C | 35 MPa Show Material materials with Resistencia a la tracción of 35 MPa | ASTM D 638 | Type I, 5 mm/min |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 7.92E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 7.92E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 7.92E-5 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 7.92E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Heat deflection temperature, 1.80 MPa | 72 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 72 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |||
Relative temperature index, electrical | 60 °C Show Material materials with Relative temperature index, electrical of 60 °C | UL 746B | |||
Relative temperature index, mechanical impact | 60 °C Show Material materials with Relative temperature index, mechanical impact of 60 °C | UL 746B | |||
Relative temperature index, mechanical strength | 60 °C Show Material materials with Relative temperature index, mechanical strength of 60 °C | UL 746B | |||
Temperatura de reblandecimiento Vicat | 90 °C Show Material materials with Temperatura de reblandecimiento Vicat of 90 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94-5VB Flame Class Rating | 2.48mm | UL 94 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.5 - 0.7 % Show Material materials with Contracción of 0.5 - 0.7 % | SABIC method | 3.2 mm |
Melt viscosity | 23.0 °C | 310 Pa·s Show Material materials with Melt viscosity of 310 Pa·s | ASTM D 3825 | 200°C, 1000 sec⁻¹ |
Velocidad de flujo de la masa derretida | 9 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 9 g/10min | ISO 1133 | 220°C/5.0 kg | |
Velocidad de flujo del volumen derretido | 37 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 37 cm³/10min | ISO 1133 | 220°C/10.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Air Conditioning,ATM/Ticket Machine,Circuit Protection,Data Transfer,Document Handling,Electronic Components,Enclosures,Furnace/Heater,Heavy Vehicles,LED Lighting,Medical Device,Medical Facility Infrastructure,Monitoring and Imaging,Personal Computing,Pharmaceutical Packaging & Drug Delivery,Power Manangement,Respiratory,Small Appliance,Wireless Communications,Wiring Devices |