DEF STAN 02-835 Copper Alloy

Want to keep this datasheet? Save it now in your required format

Description

DEF STAN 02-835 Copper Alloy is a hot forged, stress relieved high strength cupronickel developed primarily for marine and offshore applications. The alloy contains around 14.5% nickel, 4.5% manganese and smaller additions of aluminium and iron to increase the overall material strength and corrosion resistance. Specified as an MoD (Navy) grade, it combines the inherent corrosion resistance and antibiofouling benefits of traditional cupronickels whilst offering higher strength and toughness levels than the aluminium bronzes. It shows the following features and properties:


  • High strength
  • Excellent corrosion and biofouling resistance
  • High impact strength retained down to cryogenic temperatures
  • Spark resistance
  • Related Standards

    Equivalent Materials

    Los datos sobre este material han sido proporcionados por Matmatch.

    A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
    Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

    Ashby charts

    Propiedades

    General

    PropertyTemperatureValue

    Densidad

    23.0 °C

    8.53 g/cm³

    Show Material materials with Densidad of 8.53 g/cm³

    Mecánica

    PropertyTemperatureValue

    Charpy impact energy, V-notch

    23.0 °C

    40 J

    Show Material materials with Charpy impact energy, V-notch of 40 J

    Elongación

    23.0 °C

    18 - 22 %

    Show Material materials with Elongación of 18 - 22 %

    Límite elástico Rp 0,2

    23.0 °C

    400 - 430 MPa

    Show Material materials with Límite elástico Rp 0,2 of 400 - 430 MPa

    Resistencia a la tracción

    23.0 °C

    710 - 725 MPa

    Show Material materials with Resistencia a la tracción of 710 - 725 MPa

    Aplicaciones térmicas

    PropertyTemperatureValueComment

    Coeficiente de dilatación térmica

    23.0 °C

    1.6E-5 1/K

    Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 1/K

    for 0-400°C

    Conductividad térmica

    23.0 °C

    25 W/(m·K)

    Show Material materials with Conductividad térmica of 25 W/(m·K)

    Temperatura de fusión

    1030 - 1085 °C

    Show Material materials with Temperatura de fusión of 1030 - 1085 °C

    Eléctrico

    PropertyTemperatureValue

    Resistividad eléctrica

    23.0 °C

    3.5E-7 Ω·m

    Show Material materials with Resistividad eléctrica of 3.5E-7 Ω·m

    Magnético

    PropertyTemperatureValueComment

    Permeabilidad magnética relativa

    23.0 °C

    1.01 [-]

    Show Material materials with Permeabilidad magnética relativa of 1.01 [-]

    max.

    Chemical properties

    PropertyValueComment

    Aluminio

    1 - 2 %

    Show Material materials with Aluminio of 1 - 2 %

    Cobre

    Balance

    Cromo

    0.5 %

    Show Material materials with Cromo of 0.5 %

    Hierro

    0.7 - 1.2 %

    Show Material materials with Hierro of 0.7 - 1.2 %

    Manganeso

    3.5 - 5.5 %

    Show Material materials with Manganeso of 3.5 - 5.5 %

    Níquel

    13.5 - 16.5 %

    Show Material materials with Níquel of 13.5 - 16.5 %

    Otro

    0.3 %

    Show Material materials with Otro of 0.3 %

    max., Inosinic acid (IMP)

    Technological properties

    Property
    Application areas

    Offshore & marine: Critical marine fasteners, gears, shafts, pipe couplings, sonar equipment, connectors, flanges and subsea components

    Corrosion properties

    Excellent corrosion and pitting resistance in marine environments

    General machinability

    Easily machined