General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8.75 g/cm³ Show Material materials with Densidad of 8.75 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Vickers | 23.0 °C | 80 [-] Show Material materials with Dureza Vickers of 80 [-] |
Elongación | 23.0 °C | 45 % Show Material materials with Elongación of 45 % |
Límite elástico Rp 0,2 | 23.0 °C | 120 MPa Show Material materials with Límite elástico Rp 0,2 of 120 MPa |
Módulo elástico | 23.0 °C | 135 GPa Show Material materials with Módulo elástico of 135 GPa |
Resistencia a la tracción | 23.0 °C | 390 MPa Show Material materials with Resistencia a la tracción of 390 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Conductividad térmica | 23.0 °C | 25 W/(m·K) Show Material materials with Conductividad térmica of 25 W/(m·K) |
Temperatura de fusión | 1060 - 1110 °C Show Material materials with Temperatura de fusión of 1060 - 1110 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | 23.0 °C | 3.48E+6 S/m Show Material materials with Conductividad eléctrica of 3.48E+6 S/m |
Resistividad eléctrica | 23.0 °C | 2.9E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.9E-7 Ω·m |
Specific Electrical conductivity | 6 % IACS Show Material materials with Specific Electrical conductivity of 6 % IACS |
Magnético
Property | Temperature | Value | Comment |
---|---|---|---|
Permeabilidad magnética relativa | 23.0 °C | 1.05 [-] Show Material materials with Permeabilidad magnética relativa of 1.05 [-] | max. |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Cobre | 60 - 65 % Show Material materials with Cobre of 60 - 65 % | ||
Hierro | 0.3 % Show Material materials with Hierro of 0.3 % | max. | |
Manganeso | 0.05 - 0.5 % Show Material materials with Manganeso of 0.05 - 0.5 % | ||
Níquel | 17 - 19 % Show Material materials with Níquel of 17 - 19 % | ||
Plomo | 0.03 % Show Material materials with Plomo of 0.03 % | max. | |
Zinc | Balance |
Technological properties
Property | ||
---|---|---|
Application areas | General: Architectural metalwork, panels and trim, holloware, musical instruments, medals and medallions, costume jewellery, nameplates, cosmetic cases, lamp caps, lighting fittings, platters, bowls, dials, relay and contact springs, medical, industrial and scientific instrument components | |
Cold Forming | Very good cold working characteristics | |