General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8.05 g/cm³ Show Material materials with Densidad of 8.05 g/cm³ |
Medidas
Property | Value |
---|---|
Ancho | 609.6 mm Show Material materials with Ancho of 609.6 mm |
Espesor | 0.76 - 3.18 mm Show Material materials with Espesor of 0.76 - 3.18 mm |
Longitud | 1828 mm Show Material materials with Longitud of 1828 mm |
Dimensions | Available thicknesses: 0.8mm, 1.0mm, 1.6mm, 2.5mm, 3.2mm |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
Dureza Rockwell B | 23.0 °C | 80 [-] Show Material materials with Dureza Rockwell B of 80 [-] | |
Elongación | 23.0 °C | 34 % Show Material materials with Elongación of 34 % | in 2 in. |
Límite elástico | 23.0 °C | 276 MPa Show Material materials with Límite elástico of 276 MPa | |
Módulo elástico | 23.0 °C | 141 GPa Show Material materials with Módulo elástico of 141 GPa | |
Resistencia a la tracción | 23.0 °C | 518 MPa Show Material materials with Resistencia a la tracción of 518 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 502 J/(kg·K) Show Material materials with Calor específico of 502 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.9E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 1.9E-6 1/K | from 20°C to the mentioned temperature |
150.0 °C | 2.4E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4E-6 1/K | from 20°C to the mentioned temperature | |
200.0 °C | 3E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 3E-6 1/K | from 20°C to the mentioned temperature | |
250.0 °C | 4.4E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 4.4E-6 1/K | from 20°C to the mentioned temperature | |
300.0 °C | 6.1E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 6.1E-6 1/K | from 20°C to the mentioned temperature | |
350.0 °C | 7.5E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 7.5E-6 1/K | from 20°C to the mentioned temperature | |
400.0 °C | 8.7E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 8.7E-6 1/K | from 20°C to the mentioned temperature | |
450.0 °C | 8.9E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 8.9E-6 1/K | from 20°C to the mentioned temperature | |
500.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | from 20°C to the mentioned temperature | |
600.0 °C | 1.18E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.18E-5 1/K | from 20°C to the mentioned temperature | |
Conductividad térmica | 23.0 °C | 10 W/(m·K) Show Material materials with Conductividad térmica of 10 W/(m·K) | |
Temperatura de fusión | 1427 °C Show Material materials with Temperatura de fusión of 1427 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 23.0 °C | 8.2E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.2E-7 Ω·m |
Magnético
Property | Value |
---|---|
Temperatura de Curie | 279 °C Show Material materials with Temperatura de Curie of 279 °C |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.05 % Show Material materials with Carbono of 0.05 % |
Cobalto | 0.5 % Show Material materials with Cobalto of 0.5 % |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % |
Hierro | Balance |
Níquel | 36 % Show Material materials with Níquel of 36 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |
Technological properties
Property | ||
---|---|---|
Application areas | Positioning devices • Bimetal thermostats • Advanced composite molds for aerospace industry • Dimensionally stable instruments and optical devices • Containers for LNG tankers • Transfer lines for LNG • Echo boxes and filters for mobile telephones • Magnetic shielding • Small electrical transformers • Metrology devices • Scientific instruments • Electrical circuit breakers • Temperature regulators • Clock balance wheels • Pendulum clocks • Precision condenser blades • Radar and microwave cavity resonators • Special electronic housings • Seals, spacers, and specialized frames • High voltage transmission lines • CRT applications: shadow masks, deflection clips, and electron gun components. |