General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8.12 g/cm³ Show Material materials with Densidad of 8.12 g/cm³ |
Medidas
Property | Value |
---|---|
Ancho | 381 mm Show Material materials with Ancho of 381 mm |
Espesor | 4.8 - 7.1 mm Show Material materials with Espesor of 4.8 - 7.1 mm |
Longitud | 1828 mm Show Material materials with Longitud of 1828 mm |
Dimensions | Available thicknesses: 4.8mm, 7.1mm |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Rockwell B | 23.0 °C | 80 [-] Show Material materials with Dureza Rockwell B of 80 [-] | |
Elongación | 23.0 °C | 30 % Show Material materials with Elongación of 30 % | in 2 in. |
Límite elástico | 23.0 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | |
Módulo elástico | 23.0 °C | 148 GPa Show Material materials with Módulo elástico of 148 GPa | |
Resistencia a la tracción | 23.0 °C | 566 MPa Show Material materials with Resistencia a la tracción of 566 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 502 J/(kg·K) Show Material materials with Calor específico of 502 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 4.2E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 4.2E-6 1/K | from 30°C to the mentioned temperature |
150.0 °C | 4.2E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 4.2E-6 1/K | from 30°C to the mentioned temperature | |
200.0 °C | 4.2E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 4.2E-6 1/K | from 30°C to the mentioned temperature | |
250.0 °C | 4.2E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 4.2E-6 1/K | from 30°C to the mentioned temperature | |
300.0 °C | 4E-6 - 4.7E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 4E-6 - 4.7E-6 1/K | from 30°C to the mentioned temperature | |
325.0 °C | 4.6E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 4.6E-6 1/K | from 30°C to the mentioned temperature | |
350.0 °C | 5E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 5E-6 1/K | from 30°C to the mentioned temperature | |
375.0 °C | 5.6E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 5.6E-6 1/K | from 30°C to the mentioned temperature | |
400.0 °C | 6.1E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 6.1E-6 1/K | from 30°C to the mentioned temperature | |
425.0 °C | 6.7E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 6.7E-6 1/K | from 30°C to the mentioned temperature | |
450.0 °C | 6.7E-6 - 7.4E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 6.7E-6 - 7.4E-6 1/K | from 30°C to the mentioned temperature | |
475.0 °C | 7.7E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 7.7E-6 1/K | from 30°C to the mentioned temperature | |
500.0 °C | 8.1E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 8.1E-6 1/K | from 30°C to the mentioned temperature | |
525.0 °C | 8.5E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 8.5E-6 1/K | from 30°C to the mentioned temperature | |
550.0 °C | 8.9E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 8.9E-6 1/K | from 30°C to the mentioned temperature | |
600.0 °C | 9.6E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 9.6E-6 1/K | from 30°C to the mentioned temperature | |
700.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | from 30°C to the mentioned temperature | |
800.0 °C | 1.14E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.14E-5 1/K | from 30°C to the mentioned temperature | |
900.0 °C | 1.23E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.23E-5 1/K | from 30°C to the mentioned temperature | |
1004.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | from 30°C to the mentioned temperature | |
Conductividad térmica | 23.0 °C | 11 W/(m·K) Show Material materials with Conductividad térmica of 11 W/(m·K) | |
Temperatura de fusión | 1427 °C Show Material materials with Temperatura de fusión of 1427 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 23.0 °C | 6.8E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.8E-7 Ω·m |
Magnético
Property | Value |
---|---|
Temperatura de Curie | 380 °C Show Material materials with Temperatura de Curie of 380 °C |
Chemical properties
Property | Value |
---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % |
Carbono | 0.05 % Show Material materials with Carbono of 0.05 % |
Cromo | 0.03 % Show Material materials with Cromo of 0.03 % |
Hierro | Balance |
Níquel | 41 % Show Material materials with Níquel of 41 % |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % |
Technological properties
Property | ||
---|---|---|
Application areas | Common applications of Alloy 42: Thermostats, thermoswitches, integrated circuit lead frames, Glass to metal seals for a wide variety of electronic tubes, hermetic packages, and automotive and industrial lamps., high temperature curing of aircraft thermoset composites |