Structural Epoxy Resin T26 (EP-PCF)

Want to keep this datasheet? Save it now in your required format

Description

Т26 is a single part low viscosity epoxy infusion carbon fabric plasticized resin developed for high-loaded structures. T26 offers simple and flexible processing due to low viscosity at relatively low impregnation temperatures (110°С). T26 was developed specially for RTM and vacuum infusion molding, to produce laminates with low porosity and extremely high mechanical performance, especially in crack resistance. It shows the following features and properties:


  • One-part resin designed specifically for high-temperature infusion or RTM
  • Wide processing window > 7 hours at 110°C
  • Curing at 180°C provides glass transition temperature of 205°C
  • High wet glass transition temperature —172°C
  • Very high resistance to impact
  • Operating temperatures from –60°C to 150°C
  • Los datos sobre este material han sido proporcionados por Matmatch.

    A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
    Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

    Ashby charts

    Propiedades

    Mecánica

    PropertyTemperatureValueComment

    Módulo elástico

    23.0 °C

    66 GPa

    Show Material materials with Módulo elástico of 66 GPa

    ASTM D3039

    Módulo elástico transversal

    23.0 °C

    66 GPa

    Show Material materials with Módulo elástico transversal of 66 GPa

    ASTM D3039

    Resistencia a la compresión

    23.0 °C

    638 MPa

    Show Material materials with Resistencia a la compresión of 638 MPa

    ASTM D6641

    Resistencia a la compresión transversal

    23.0 °C

    608 MPa

    Show Material materials with Resistencia a la compresión transversal of 608 MPa

    ASTM D6641

    Resistencia a la tracción

    23.0 °C

    904 MPa

    Show Material materials with Resistencia a la tracción of 904 MPa

    ASTM D3039

    Resistencia a la tracción transversal

    23.0 °C

    904 MPa

    Show Material materials with Resistencia a la tracción transversal of 904 MPa

    ASTM D3039

    Shear modulus, G₁₂

    23.0 °C

    4.3 GPa

    Show Material materials with Shear modulus, G₁₂ of 4.3 GPa

    ASTM D5379

    Shear strength, τ₁₂

    23.0 °C

    79 MPa

    Show Material materials with Shear strength, τ₁₂ of 79 MPa

    Shear strength, τ₁₃

    25.0 °C

    66 MPa

    Show Material materials with Shear strength, τ₁₃ of 66 MPa

    ASTM D2344

    120.0 °C

    40 MPa

    Show Material materials with Shear strength, τ₁₃ of 40 MPa

    ASTM D2344

    150.0 °C

    34 MPa

    Show Material materials with Shear strength, τ₁₃ of 34 MPa

    ASTM D2344

    Liberación de energía de deformación

    ASTM D5528

    Technological properties

    Property
    Application areas

    Drones;Sports equipment: Frame, wheels, seat, seat post, handlebar, head stem and crank arm of a sports bicycle are made of carbon composite;Geometry strengthen elements: Experimental stringer panel

    Processing history

    Samples for testing were obtained by vacuum infusion based on T26 resin and plasticized carbon fabric (PCF) 22508 covered by veil.

    Processing methods

    Preheat the resin to 60-90°С in its container for transfer to the resin pot. Degas the resin for 30-40 minutes while heating to 90°С. Preheat the tool to 100-110°С (or to 115-120°С for parts having complex shape or for UD parts). Maintaining resin pot temperature of 95 °С and tool temperature of 100-115 °С, begin resin infusion. After complete impregnation increase tool temperature at 2°С/min to 180°С. Dwell at 180°С for 3 h. Cool the tool to 90°С at <5°С/min before releasing part from tool.