General
Property | Value | Shape | Related Standards |
---|---|---|---|
Densidad | 4.59 g/cm³ Show Material materials with Densidad of 4.59 g/cm³ | Bar, Billet | |
4.6 g/cm³ Show Material materials with Densidad of 4.6 g/cm³ | DIN 17851 |
Medidas
Property | Temperature | Value | Shape | Comment |
---|---|---|---|---|
Dimensions | 15-65 mm diameter up to 6000 mm length °C | 7-14.5 mm diameter up to 3000 mm length | Bar | |
Diámetro | 7 mm Show Material materials with Diámetro of 7 mm | Bar | ||
115 mm Show Material materials with Diámetro of 115 mm | Bar | |||
130 mm Show Material materials with Diámetro of 130 mm | Billet | |||
350 mm Show Material materials with Diámetro of 350 mm | Billet | |||
Longitud | 3000 mm Show Material materials with Longitud of 3000 mm | Billet | ||
4500 mm Show Material materials with Longitud of 4500 mm | Billet | |||
6000 mm Show Material materials with Longitud of 6000 mm | Bar | max |
Mecánica
Property | Temperature | Value | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dureza Brinell | 350.0 [-] Show Material materials with Dureza Brinell of 350.0 [-] | DIN 17851 | |||
Elongación | 12.0 % Show Material materials with Elongación of 12.0 % | Bar, Billet | |||
Estricción | 20.0 % Show Material materials with Estricción of 20.0 % | DIN 17851 | |||
20.0 % Show Material materials with Estricción of 20.0 % | DIN 17851 | Transverse | |||
Límite elástico | 870.0 MPa Show Material materials with Límite elástico of 870.0 MPa | DIN 17851 | RP02 | ||
920.0 MPa Show Material materials with Límite elástico of 920.0 MPa | DIN 17851 | RP02 | |||
960.0 MPa Show Material materials with Límite elástico of 960.0 MPa | DIN 17851 | RP02 | |||
1035.0 MPa Show Material materials with Límite elástico of 1035.0 MPa | Bar | ||||
1050.0 MPa Show Material materials with Límite elástico of 1050.0 MPa | DIN 17851 | RP02 | |||
Módulo elástico | 114.0 GPa Show Material materials with Módulo elástico of 114.0 GPa | Bar | |||
117.0 GPa Show Material materials with Módulo elástico of 117.0 GPa | DIN 17851 | ||||
Resistencia a la tracción | 1000.0 MPa Show Material materials with Resistencia a la tracción of 1000.0 MPa | DIN 17851 | |||
1050.0 MPa Show Material materials with Resistencia a la tracción of 1050.0 MPa | DIN 17851 | ||||
1100.0 MPa Show Material materials with Resistencia a la tracción of 1100.0 MPa | DIN 17851 | ||||
1138.0 MPa Show Material materials with Resistencia a la tracción of 1138.0 MPa | Bar, Billet | ||||
500 °C | 750.0 MPa Show Material materials with Resistencia a la tracción of 750.0 MPa | DIN 17851 |
Aplicaciones térmicas
Property | Temperature | Value | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Calor específico | 370.0 - 674.0 J/(kg·K) Show Material materials with Calor específico of 370.0 - 674.0 J/(kg·K) | Typical for Titanium Alpha Beta Alloy | |||
Coeficiente de dilatación térmica | 20 °C | 8.599999999999999e-06 1/K Show Material materials with Coeficiente de dilatación térmica of 8.599999999999999e-06 1/K | DIN 17851 | ||
200 °C | 8.599999999999999e-06 1/K Show Material materials with Coeficiente de dilatación térmica of 8.599999999999999e-06 1/K | DIN 17851 | |||
Conductividad térmica | 7.54 W/(m·K) Show Material materials with Conductividad térmica of 7.54 W/(m·K) | DIN 17851 | |||
7.6 W/(m·K) Show Material materials with Conductividad térmica of 7.6 W/(m·K) | Bar | ||||
Temperatura de fusión | 1500.0 - 1750.0 °C Show Material materials with Temperatura de fusión of 1500.0 - 1750.0 °C | Typical for Titanium Alpha Beta Alloy |
Eléctrico
Property | Value | Related Standards |
---|---|---|
Resistividad eléctrica | 1.5e-06 Show Material materials with Resistividad eléctrica of 1.5e-06 | DIN 17851 |
Chemical properties
Property | Value | Related Standards | Shape |
---|---|---|---|
Aluminio | 3.0 - 5.0 % Show Material materials with Aluminio of 3.0 - 5.0 % | DIN 17851 | Bar, Billet |
Carbono | 0.08 % Show Material materials with Carbono of 0.08 % | DIN 17851 | |
Estaño | 1.5 - 2.5 % Show Material materials with Estaño of 1.5 - 2.5 % | DIN 17851 | Bar, Billet |
Hidrógeno | 0.0125 % Show Material materials with Hidrógeno of 0.0125 % | Bar, Billet | |
0.015 % Show Material materials with Hidrógeno of 0.015 % | DIN 17851 | ||
Hierro | 0.20 % Show Material materials with Hierro of 0.20 % | DIN 17851 | |
0.2 % Show Material materials with Hierro of 0.2 % | Bar, Billet | ||
Molibdeno | 3.0 - 5.0 % Show Material materials with Molibdeno of 3.0 - 5.0 % | DIN 17851 | Bar, Billet |
Nitrógeno | 0.05 % Show Material materials with Nitrógeno of 0.05 % | DIN 17851 | Bar, Billet |
Oxígeno | 0.25 % Show Material materials with Oxígeno of 0.25 % | DIN 17851 | |
0.27 % Show Material materials with Oxígeno of 0.27 % | Bar, Billet | ||
Silicona | 0.3 - 0.7 % Show Material materials with Silicona of 0.3 - 0.7 % | DIN 17851 | Bar, Billet |