General
Property | Value | Shape | Related Standards |
---|---|---|---|
Densidad | 4.49 g/cm³ Show Material materials with Densidad of 4.49 g/cm³ | Billet | |
4.505 g/cm³ Show Material materials with Densidad of 4.505 g/cm³ | Tube | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 |
Medidas
Property | Value | Related Standards | Shape |
---|---|---|---|
Diámetro | 5 mm Show Material materials with Diámetro of 5 mm | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Tube |
25.4 mm Show Material materials with Diámetro of 25.4 mm | Billet | ||
125 mm Show Material materials with Diámetro of 125 mm | Billet | ||
130 mm Show Material materials with Diámetro of 130 mm | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Tube | |
Longitud | 1000 mm Show Material materials with Longitud of 1000 mm | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Tube |
5000 mm Show Material materials with Longitud of 5000 mm | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Tube | |
Wall thickness | 0.5 - 9.0 mm Show Material materials with Wall thickness of 0.5 - 9.0 mm | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Tube |
2.5 - 21.0 mm Show Material materials with Wall thickness of 2.5 - 21.0 mm | Billet |
Mecánica
Property | Value | Related Standards | Shape | Comment |
---|---|---|---|---|
Elongación | 10.0 - 30.0 % Show Material materials with Elongación of 10.0 - 30.0 % | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Tube | |
15.0 - 25.0 % Show Material materials with Elongación of 15.0 - 25.0 % | Billet | |||
Límite elástico | 380.0 - 550.0 MPa Show Material materials with Límite elástico of 380.0 - 550.0 MPa | Billet | ||
Módulo elástico | 100.0 - 120.0 GPa Show Material materials with Módulo elástico of 100.0 - 120.0 GPa | Typical for Titanium Alpha Alloy | ||
Resistencia a la tracción | 295.0 - 590.0 MPa Show Material materials with Resistencia a la tracción of 295.0 - 590.0 MPa | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Tube | |
480.0 - 680.0 MPa Show Material materials with Resistencia a la tracción of 480.0 - 680.0 MPa | Billet |
Aplicaciones térmicas
Property | Temperature | Value | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Calor específico | 460.0 - 527.0 J/(kg·K) Show Material materials with Calor específico of 460.0 - 527.0 J/(kg·K) | Typical for Titanium Alpha Alloy | |||
Coeficiente de dilatación térmica | 7.599999999999997e-06 - 1.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 7.599999999999997e-06 - 1.1e-05 1/K | Typical for Titanium Alpha Alloy | |||
Conductividad térmica | 10 W/(m·K) Show Material materials with Conductividad térmica of 10 W/(m·K) | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube | ||
100 °C | 9.3 W/(m·K) Show Material materials with Conductividad térmica of 9.3 W/(m·K) | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube | ||
200 °C | 5 W/(m·K) Show Material materials with Conductividad térmica of 5 W/(m·K) | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube | ||
300 °C | 11.9 W/(m·K) Show Material materials with Conductividad térmica of 11.9 W/(m·K) | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube | ||
300 °C | 11.9 W/(m·K) Show Material materials with Conductividad térmica of 11.9 W/(m·K) | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube | ||
400 °C | 13.3 W/(m·K) Show Material materials with Conductividad térmica of 13.3 W/(m·K) | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube | ||
400 °C | 13.3 W/(m·K) Show Material materials with Conductividad térmica of 13.3 W/(m·K) | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube | ||
Temperatura de fusión | 1668.0 °C Show Material materials with Temperatura de fusión of 1668.0 °C | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Tube |
Chemical properties
Property | Value | Related Standards | Shape |
---|---|---|---|
Aluminio | 1.8 - 2.5 % Show Material materials with Aluminio of 1.8 - 2.5 % | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube |
Carbono | 0.1 Show Material materials with Carbono of 0.1 | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube |
Circonio | 2.0 - 3.0 % Show Material materials with Circonio of 2.0 - 3.0 % | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube |
Nitrógeno | 0.04 Show Material materials with Nitrógeno of 0.04 | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube |
Silicona | 0.12 Show Material materials with Silicona of 0.12 | GOST 22178, ОSТ 190218, ТU 1-92-89, ТU 1-5-356 | Billet, Tube |