General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 7.72 g/cm³ Show Material materials with Densidad of 7.72 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación | 23.0 °C | 20 % Show Material materials with Elongación of 20 % | |
Estricción | 20.0 °C | 15 % Show Material materials with Estricción of 15 % | |
650.0 °C | 48 % Show Material materials with Estricción of 48 % | ||
760.0 °C | 14 % Show Material materials with Estricción of 14 % | ||
Límite elástico | 20.0 °C | 520 MPa Show Material materials with Límite elástico of 520 MPa | |
650.0 °C | 260 MPa Show Material materials with Límite elástico of 260 MPa | ||
760.0 °C | 210 MPa Show Material materials with Límite elástico of 210 MPa | ||
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | 23.0 °C | 195 GPa Show Material materials with Módulo elástico of 195 GPa | Typical for Austenitic Stainless Steel |
Resistencia a la tracción | 20.0 °C | 1030 MPa Show Material materials with Resistencia a la tracción of 1030 MPa | |
650.0 °C | 500 MPa Show Material materials with Resistencia a la tracción of 500 MPa | ||
760.0 °C | 340 MPa Show Material materials with Resistencia a la tracción of 340 MPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | Typical for Austenitic Stainless Steel |
Coeficiente de dilatación térmica | 760.0 °C | 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K | The mentioned value is between 20°C and the mentioned temperature |
Conductividad térmica | 23.0 °C | 11 - 21 W/(m·K) Show Material materials with Conductividad térmica of 11 - 21 W/(m·K) | Typical for Austenitic Stainless Steel |
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Resistividad eléctrica | 23.0 °C | 8.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value | Comment |
---|---|---|
Azufre | 0.025 - 0.065 % Show Material materials with Azufre of 0.025 - 0.065 % | |
Carbono | 0.65 - 0.75 % Show Material materials with Carbono of 0.65 - 0.75 % | |
Cromo | 20 - 22 % Show Material materials with Cromo of 20 - 22 % | |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % | |
Hierro | 67.22 - 71.82 % Show Material materials with Hierro of 67.22 - 71.82 % | Balance |
Manganeso | 5.5 - 7 % Show Material materials with Manganeso of 5.5 - 7 % | |
Nitrógeno | 0.18 - 0.28 % Show Material materials with Nitrógeno of 0.18 - 0.28 % | |
Níquel | 1.4 - 1.9 % Show Material materials with Níquel of 1.4 - 1.9 % | |
Silicona | 0.45 - 0.85 % Show Material materials with Silicona of 0.45 - 0.85 % |