General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | normalized or normalized formed (+N) | EN 10084, ISO 683-3 | Bar, Flat, Forging, Wire | |
Elongación | 14.7 % Show Material materials with Elongación of 14.7 % | Predicted Value, A80 | ||||
15.5 % Show Material materials with Elongación of 15.5 % | Predicted Value, A200 | |||||
16.5 % Show Material materials with Elongación of 16.5 % | Predicted Value, Transverse | |||||
17.8 % Show Material materials with Elongación of 17.8 % | Predicted Value, A50 | |||||
17.8 % Show Material materials with Elongación of 17.8 % | Predicted Value, A80 Transverse | |||||
18.4 % Show Material materials with Elongación of 18.4 % | Predicted Value, A5 | |||||
20.9 % Show Material materials with Elongación of 20.9 % | Predicted Value | |||||
Estricción | 41.4 % Show Material materials with Estricción of 41.4 % | Predicted Value, Transverse | ||||
47.2 % Show Material materials with Estricción of 47.2 % | Predicted Value | |||||
Módulo de cizallamiento | 20 °C | 81 GPa Show Material materials with Módulo de cizallamiento of 81 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 210 - 212 GPa Show Material materials with Módulo elástico of 210 - 212 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 210 GPa Show Material materials with Módulo elástico of 210 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 188 - 199 GPa Show Material materials with Módulo elástico of 188 - 199 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 188 GPa Show Material materials with Módulo elástico of 188 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
Resistencia al cizallamiento | 514.2 MPa Show Material materials with Resistencia al cizallamiento of 514.2 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 460 - 461 J/(kg·K) Show Material materials with Calor específico of 460 - 461 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 460 J/(kg·K) Show Material materials with Calor específico of 460 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
Coeficiente de dilatación térmica | -100 °C | 1.05e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 1.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 1.1e-05 - 1.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1e-05 - 1.21e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 1.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 1.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 1.27e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 1.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 1.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44e-05 1/K | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
Conductividad térmica | 20 °C | 42 - 45.9 W/(m·K) Show Material materials with Conductividad térmica of 42 - 45.9 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 42 W/(m·K) Show Material materials with Conductividad térmica of 42 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 45.9 W/(m·K) Show Material materials with Conductividad térmica of 45.9 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 39.8 - 46.4 W/(m·K) Show Material materials with Conductividad térmica of 39.8 - 46.4 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 39.8 W/(m·K) Show Material materials with Conductividad térmica of 39.8 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 46.4 W/(m·K) Show Material materials with Conductividad térmica of 46.4 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 37.7 - 45.6 W/(m·K) Show Material materials with Conductividad térmica of 37.7 - 45.6 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 37.7 W/(m·K) Show Material materials with Conductividad térmica of 37.7 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 45.6 W/(m·K) Show Material materials with Conductividad térmica of 45.6 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 43.5 W/(m·K) Show Material materials with Conductividad térmica of 43.5 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 40.9 W/(m·K) Show Material materials with Conductividad térmica of 40.9 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 38.2 W/(m·K) Show Material materials with Conductividad térmica of 38.2 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 35.5 W/(m·K) Show Material materials with Conductividad térmica of 35.5 W/(m·K) | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
Difusividad térmica | 20 °C | 12.7 mm²/s Show Material materials with Difusividad térmica of 12.7 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
100 °C | 12 mm²/s Show Material materials with Difusividad térmica of 12 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 11 mm²/s Show Material materials with Difusividad térmica of 11 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 9.9 mm²/s Show Material materials with Difusividad térmica of 9.9 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 8.7 mm²/s Show Material materials with Difusividad térmica of 8.7 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 7.3 mm²/s Show Material materials with Difusividad térmica of 7.3 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 4 S/m Show Material materials with Conductividad eléctrica of 4 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 1.6e-07 - 2.27e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.6e-07 - 2.27e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | |
20 °C | 1.6e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.6e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
20 °C | 2.27e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.27e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
100 °C | 2.76e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.76e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
200 °C | 3.46e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.46e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
300 °C | 4.31e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.31e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
400 °C | 5.32e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.32e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
500 °C | 6.48e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.48e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire | ||
600 °C | 7.81e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.81e-07 Ω·m | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Carbono | 0.14 - 0.19 % Show Material materials with Carbono of 0.14 - 0.19 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Cobre | 0.4 % Show Material materials with Cobre of 0.4 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Cromo | 0.8 - 1.1 % Show Material materials with Cromo of 0.8 - 1.1 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Manganeso | 1 - 1.3 % Show Material materials with Manganeso of 1 - 1.3 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
Silicona | 0.15 - 0.4 % Show Material materials with Silicona of 0.15 - 0.4 % | normalized or normalized formed (+N) | ISO 683-3, EN 10084 | Bar, Flat, Forging, Wire |
0.4 % Show Material materials with Silicona of 0.4 % | normalized or normalized formed (+N) | EN 10084, ISO 683-3 | Bar, Flat, Forging, Wire |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |