General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.1 g/cm³ Show Material materials with Densidad of 8.1 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 217 [-] Show Material materials with Dureza Brinell of 217 [-] |
Elongación | 20.0 °C | 30 % Show Material materials with Elongación of 30 % |
100.0 °C | 40 % Show Material materials with Elongación of 40 % | |
200.0 °C | 40 % Show Material materials with Elongación of 40 % | |
300.0 °C | 40 % Show Material materials with Elongación of 40 % | |
Estricción | 20.0 °C | 50 % Show Material materials with Estricción of 50 % |
Límite elástico Rp 0,2 | 20.0 °C | 240 MPa Show Material materials with Límite elástico Rp 0,2 of 240 MPa |
100.0 °C | 210 MPa Show Material materials with Límite elástico Rp 0,2 of 210 MPa | |
200.0 °C | 180 MPa Show Material materials with Límite elástico Rp 0,2 of 180 MPa | |
300.0 °C | 140 MPa Show Material materials with Límite elástico Rp 0,2 of 140 MPa | |
Módulo elástico | 20.0 °C | 195 GPa Show Material materials with Módulo elástico of 195 GPa |
Resistencia a la tracción | 20.0 °C | 550 MPa Show Material materials with Resistencia a la tracción of 550 MPa |
100.0 °C | 520 MPa Show Material materials with Resistencia a la tracción of 520 MPa | |
200.0 °C | 500 MPa Show Material materials with Resistencia a la tracción of 500 MPa | |
300.0 °C | 480 MPa Show Material materials with Resistencia a la tracción of 480 MPa | |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.5E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.5E-5 1/K | |
200.0 °C | 1.57E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.57E-5 1/K | ||
300.0 °C | 1.63E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.63E-5 1/K | ||
400.0 °C | 1.68E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.68E-5 1/K | ||
500.0 °C | 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.72E-5 1/K | ||
600.0 °C | 1.74E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.74E-5 1/K | ||
700.0 °C | 1.76E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.76E-5 1/K | ||
800.0 °C | 1.78E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.78E-5 1/K | ||
Conductividad térmica | 20.0 °C | 12.3 W/(m·K) Show Material materials with Conductividad térmica of 12.3 W/(m·K) | |
100.0 °C | 13.1 W/(m·K) Show Material materials with Conductividad térmica of 13.1 W/(m·K) | ||
200.0 °C | 14.8 W/(m·K) Show Material materials with Conductividad térmica of 14.8 W/(m·K) | ||
300.0 °C | 16.5 W/(m·K) Show Material materials with Conductividad térmica of 16.5 W/(m·K) | ||
400.0 °C | 18.1 W/(m·K) Show Material materials with Conductividad térmica of 18.1 W/(m·K) | ||
500.0 °C | 19.7 W/(m·K) Show Material materials with Conductividad térmica of 19.7 W/(m·K) | ||
600.0 °C | 21 W/(m·K) Show Material materials with Conductividad térmica of 21 W/(m·K) | ||
Temperatura de fusión | 1200 - 1480 °C Show Material materials with Temperatura de fusión of 1200 - 1480 °C | Typical for Nickel Chromium Iron Alloy | |
Temperatura máx. de funcionamiento, largo | 0 - 500 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 500 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 Ω·m |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.07 % Show Material materials with Carbono of 0.07 % |
Cobalto | 1.5 % Show Material materials with Cobalto of 1.5 % |
Cobre | 3 - 4 % Show Material materials with Cobre of 3 - 4 % |
Cromo | 19 - 21 % Show Material materials with Cromo of 19 - 21 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Hierro | 28.4 % Show Material materials with Hierro of 28.4 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 2 - 3 % Show Material materials with Molibdeno of 2 - 3 % |
Níquel | 32 - 38 % Show Material materials with Níquel of 32 - 38 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |