General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.05 - 8.1 g/cm³ Show Material materials with Densidad of 8.05 - 8.1 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 190 - 210 [-] Show Material materials with Dureza Brinell of 190 - 210 [-] |
Elongación | 20.0 °C | 30 - 35 % Show Material materials with Elongación of 30 - 35 % |
Elongación transversal | 20.0 °C | 30 % Show Material materials with Elongación transversal of 30 % |
Elongation A100 | 20.0 °C | 20 - 30 % Show Material materials with Elongation A100 of 20 - 30 % |
Límite elástico Rp 0,2 | 20.0 °C | 220 - 240 MPa Show Material materials with Límite elástico Rp 0,2 of 220 - 240 MPa |
100.0 °C | 190 - 205 MPa Show Material materials with Límite elástico Rp 0,2 of 190 - 205 MPa | |
150.0 °C | 175 - 190 MPa Show Material materials with Límite elástico Rp 0,2 of 175 - 190 MPa | |
200.0 °C | 165 - 180 MPa Show Material materials with Límite elástico Rp 0,2 of 165 - 180 MPa | |
250.0 °C | 160 - 175 MPa Show Material materials with Límite elástico Rp 0,2 of 160 - 175 MPa | |
300.0 °C | 155 - 170 MPa Show Material materials with Límite elástico Rp 0,2 of 155 - 170 MPa | |
350.0 °C | 150 - 165 MPa Show Material materials with Límite elástico Rp 0,2 of 150 - 165 MPa | |
400.0 °C | 145 - 160 MPa Show Material materials with Límite elástico Rp 0,2 of 145 - 160 MPa | |
450.0 °C | 140 - 155 MPa Show Material materials with Límite elástico Rp 0,2 of 140 - 155 MPa | |
Límite elástico Rp 1,0 | 20.0 °C | 250 - 270 MPa Show Material materials with Límite elástico Rp 1,0 of 250 - 270 MPa |
100.0 °C | 220 - 235 MPa Show Material materials with Límite elástico Rp 1,0 of 220 - 235 MPa | |
150.0 °C | 205 - 220 MPa Show Material materials with Límite elástico Rp 1,0 of 205 - 220 MPa | |
200.0 °C | 190 - 205 MPa Show Material materials with Límite elástico Rp 1,0 of 190 - 205 MPa | |
250.0 °C | 185 - 200 MPa Show Material materials with Límite elástico Rp 1,0 of 185 - 200 MPa | |
300.0 °C | 180 - 195 MPa Show Material materials with Límite elástico Rp 1,0 of 180 - 195 MPa | |
350.0 °C | 175 - 190 MPa Show Material materials with Límite elástico Rp 1,0 of 175 - 190 MPa | |
400.0 °C | 170 - 185 MPa Show Material materials with Límite elástico Rp 1,0 of 170 - 185 MPa | |
450.0 °C | 165 - 180 MPa Show Material materials with Límite elástico Rp 1,0 of 165 - 180 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 220 - 235 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 220 - 235 MPa |
Límite elástico transversal Rp 1,0 | 20.0 °C | 250 - 265 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 250 - 265 MPa |
Módulo elástico | 20.0 °C | 195 GPa Show Material materials with Módulo elástico of 195 GPa |
100.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | |
200.0 °C | 185 GPa Show Material materials with Módulo elástico of 185 GPa | |
300.0 °C | 179 GPa Show Material materials with Módulo elástico of 179 GPa | |
400.0 °C | 174 GPa Show Material materials with Módulo elástico of 174 GPa | |
500.0 °C | 168 GPa Show Material materials with Módulo elástico of 168 GPa | |
600.0 °C | 161 GPa Show Material materials with Módulo elástico of 161 GPa | |
700.0 °C | 154 GPa Show Material materials with Módulo elástico of 154 GPa | |
800.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | |
900.0 °C | 130 GPa Show Material materials with Módulo elástico of 130 GPa | |
1000.0 °C | 119 GPa Show Material materials with Módulo elástico of 119 GPa | |
Resistencia a la tracción | 20.0 °C | 500 - 750 MPa Show Material materials with Resistencia a la tracción of 500 - 750 MPa |
100.0 °C | 520 - 530 MPa Show Material materials with Resistencia a la tracción of 520 - 530 MPa | |
200.0 °C | 490 - 515 MPa Show Material materials with Resistencia a la tracción of 490 - 515 MPa | |
300.0 °C | 480 - 500 MPa Show Material materials with Resistencia a la tracción of 480 - 500 MPa | |
400.0 °C | 470 - 490 MPa Show Material materials with Resistencia a la tracción of 470 - 490 MPa | |
450.0 °C | 465 - 485 MPa Show Material materials with Resistencia a la tracción of 465 - 485 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 550 - 750 MPa Show Material materials with Resistencia a la tracción transversal of 550 - 750 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
100.0 °C | 462 J/(kg·K) Show Material materials with Calor específico of 462 J/(kg·K) | ||
200.0 °C | 488 J/(kg·K) Show Material materials with Calor específico of 488 J/(kg·K) | ||
300.0 °C | 514 J/(kg·K) Show Material materials with Calor específico of 514 J/(kg·K) | ||
400.0 °C | 540 J/(kg·K) Show Material materials with Calor específico of 540 J/(kg·K) | ||
500.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
600.0 °C | 590 J/(kg·K) Show Material materials with Calor específico of 590 J/(kg·K) | ||
700.0 °C | 615 J/(kg·K) Show Material materials with Calor específico of 615 J/(kg·K) | ||
800.0 °C | 655 J/(kg·K) Show Material materials with Calor específico of 655 J/(kg·K) | ||
900.0 °C | 680 J/(kg·K) Show Material materials with Calor específico of 680 J/(kg·K) | ||
1000.0 °C | 710 J/(kg·K) Show Material materials with Calor específico of 710 J/(kg·K) | ||
Coeficiente de dilatación térmica | 100.0 °C | 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41E-5 1/K | |
200.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | ||
300.0 °C | 1.52E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.52E-5 1/K | ||
400.0 °C | 1.56E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.56E-5 1/K | ||
500.0 °C | 1.58E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.58E-5 1/K | ||
600.0 °C | 1.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 1/K | ||
700.0 °C | 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.67E-5 1/K | ||
800.0 °C | 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.72E-5 1/K | ||
900.0 °C | 1.76E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.76E-5 1/K | ||
1000.0 °C | 1.79E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.79E-5 1/K | ||
Conductividad térmica | 20.0 °C | 10.8 W/(m·K) Show Material materials with Conductividad térmica of 10.8 W/(m·K) | |
100.0 °C | 12.4 W/(m·K) Show Material materials with Conductividad térmica of 12.4 W/(m·K) | ||
200.0 °C | 14.1 W/(m·K) Show Material materials with Conductividad térmica of 14.1 W/(m·K) | ||
300.0 °C | 15.6 W/(m·K) Show Material materials with Conductividad térmica of 15.6 W/(m·K) | ||
400.0 °C | 16.9 W/(m·K) Show Material materials with Conductividad térmica of 16.9 W/(m·K) | ||
500.0 °C | 18.3 W/(m·K) Show Material materials with Conductividad térmica of 18.3 W/(m·K) | ||
600.0 °C | 19.6 W/(m·K) Show Material materials with Conductividad térmica of 19.6 W/(m·K) | ||
700.0 °C | 21 W/(m·K) Show Material materials with Conductividad térmica of 21 W/(m·K) | ||
800.0 °C | 23.2 W/(m·K) Show Material materials with Conductividad térmica of 23.2 W/(m·K) | ||
900.0 °C | 25.7 W/(m·K) Show Material materials with Conductividad térmica of 25.7 W/(m·K) | ||
1000.0 °C | 28.1 W/(m·K) Show Material materials with Conductividad térmica of 28.1 W/(m·K) | ||
Temperatura de fusión | 1200 - 1480 °C Show Material materials with Temperatura de fusión of 1200 - 1480 °C | Typical for Nickel Chromium Iron Alloy | |
Temperatura máx. de funcionamiento, largo | -10 - 450 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -10 - 450 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m |
100.0 °C | 1.14E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.14E-6 Ω·m | |
200.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
300.0 °C | 1.2E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.2E-6 Ω·m | |
400.0 °C | 1.24E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.24E-6 Ω·m | |
500.0 °C | 1.26E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.26E-6 Ω·m | |
600.0 °C | 1.26E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.26E-6 Ω·m | |
700.0 °C | 1.27E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.27E-6 Ω·m | |
800.0 °C | 1.28E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.28E-6 Ω·m | |
900.0 °C | 1.29E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.29E-6 Ω·m | |
1000.0 °C | 1.3E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.3E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.2 % Show Material materials with Aluminio of 0.2 % |
Azufre | 0.01 - 0.015 % Show Material materials with Azufre of 0.01 - 0.015 % |
Carbono | 0.025 % Show Material materials with Carbono of 0.025 % |
Cobalto | 1 % Show Material materials with Cobalto of 1 % |
Cobre | 1.5 - 3 % Show Material materials with Cobre of 1.5 - 3 % |
Cromo | 19.5 - 23.5 % Show Material materials with Cromo of 19.5 - 23.5 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Hierro | 20.04 % Show Material materials with Hierro of 20.04 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Molibdeno | 2.5 - 3.5 % Show Material materials with Molibdeno of 2.5 - 3.5 % |
Níquel | 38 - 46 % Show Material materials with Níquel of 38 - 46 % |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % |
Titanio | 0.6 - 1.2 % Show Material materials with Titanio of 0.6 - 1.2 % |