General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.8 - 8.82 g/cm³ Show Material materials with Densidad of 8.8 - 8.82 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 140 - 150 [-] Show Material materials with Dureza Brinell of 140 - 150 [-] |
Dureza Vickers 10 | 20.0 °C | 155 [-] Show Material materials with Dureza Vickers 10 of 155 [-] |
Elongación | 20.0 °C | 30 - 35 % Show Material materials with Elongación of 30 - 35 % |
100.0 °C | 30 % Show Material materials with Elongación of 30 % | |
200.0 °C | 30 % Show Material materials with Elongación of 30 % | |
300.0 °C | 30 % Show Material materials with Elongación of 30 % | |
400.0 °C | 30 % Show Material materials with Elongación of 30 % | |
425.0 °C | 30 % Show Material materials with Elongación of 30 % | |
Elongación A50 | 20.0 °C | 30 % Show Material materials with Elongación A50 of 30 % |
Elongation A100 | 20.0 °C | 20 - 30 % Show Material materials with Elongation A100 of 20 - 30 % |
Límite elástico Rp 0,2 | 20.0 °C | 150 - 180 MPa Show Material materials with Límite elástico Rp 0,2 of 150 - 180 MPa |
100.0 °C | 150 MPa Show Material materials with Límite elástico Rp 0,2 of 150 MPa | |
150.0 °C | 140 MPa Show Material materials with Límite elástico Rp 0,2 of 140 MPa | |
200.0 °C | 135 MPa Show Material materials with Límite elástico Rp 0,2 of 135 MPa | |
250.0 °C | 132 MPa Show Material materials with Límite elástico Rp 0,2 of 132 MPa | |
300.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | |
350.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | |
400.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | |
425.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | |
Límite elástico Rp 1,0 | 20.0 °C | 205 - 210 MPa Show Material materials with Límite elástico Rp 1,0 of 205 - 210 MPa |
100.0 °C | 220 MPa Show Material materials with Límite elástico Rp 1,0 of 220 MPa | |
200.0 °C | 210 MPa Show Material materials with Límite elástico Rp 1,0 of 210 MPa | |
300.0 °C | 190 MPa Show Material materials with Límite elástico Rp 1,0 of 190 MPa | |
400.0 °C | 180 MPa Show Material materials with Límite elástico Rp 1,0 of 180 MPa | |
Límite elástico transversal Rp 0,2 | 100.0 °C | 150 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 150 MPa |
150.0 °C | 140 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 140 MPa | |
200.0 °C | 135 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 135 MPa | |
250.0 °C | 132 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 132 MPa | |
300.0 °C | 130 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 130 MPa | |
350.0 °C | 130 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 130 MPa | |
400.0 °C | 130 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 130 MPa | |
425.0 °C | 130 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 130 MPa | |
Módulo elástico | 20.0 °C | 182 GPa Show Material materials with Módulo elástico of 182 GPa |
100.0 °C | 180 GPa Show Material materials with Módulo elástico of 180 GPa | |
200.0 °C | 177 GPa Show Material materials with Módulo elástico of 177 GPa | |
300.0 °C | 170 GPa Show Material materials with Módulo elástico of 170 GPa | |
400.0 °C | 165 GPa Show Material materials with Módulo elástico of 165 GPa | |
500.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | |
Resistencia a la tracción | 20.0 °C | 400 - 730 MPa Show Material materials with Resistencia a la tracción of 400 - 730 MPa |
100.0 °C | 420 MPa Show Material materials with Resistencia a la tracción of 420 MPa | |
150.0 °C | 400 MPa Show Material materials with Resistencia a la tracción of 400 MPa | |
200.0 °C | 390 MPa Show Material materials with Resistencia a la tracción of 390 MPa | |
250.0 °C | 385 MPa Show Material materials with Resistencia a la tracción of 385 MPa | |
300.0 °C | 380 MPa Show Material materials with Resistencia a la tracción of 380 MPa | |
350.0 °C | 375 MPa Show Material materials with Resistencia a la tracción of 375 MPa | |
400.0 °C | 370 MPa Show Material materials with Resistencia a la tracción of 370 MPa | |
425.0 °C | 360 - 370 MPa Show Material materials with Resistencia a la tracción of 360 - 370 MPa | |
Resistencia a la tracción transversal | 100.0 °C | 420 MPa Show Material materials with Resistencia a la tracción transversal of 420 MPa |
150.0 °C | 400 MPa Show Material materials with Resistencia a la tracción transversal of 400 MPa | |
200.0 °C | 390 MPa Show Material materials with Resistencia a la tracción transversal of 390 MPa | |
250.0 °C | 385 MPa Show Material materials with Resistencia a la tracción transversal of 385 MPa | |
300.0 °C | 380 MPa Show Material materials with Resistencia a la tracción transversal of 380 MPa | |
350.0 °C | 375 MPa Show Material materials with Resistencia a la tracción transversal of 375 MPa | |
400.0 °C | 370 MPa Show Material materials with Resistencia a la tracción transversal of 370 MPa | |
425.0 °C | 370 MPa Show Material materials with Resistencia a la tracción transversal of 370 MPa | |
Resistencia al cizallamiento | 20.0 °C | 340 MPa Show Material materials with Resistencia al cizallamiento of 340 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 427 - 452 J/(kg·K) Show Material materials with Calor específico of 427 - 452 J/(kg·K) | |
100.0 °C | 445 - 461 J/(kg·K) Show Material materials with Calor específico of 445 - 461 J/(kg·K) | ||
200.0 °C | 465 - 473 J/(kg·K) Show Material materials with Calor específico of 465 - 473 J/(kg·K) | ||
300.0 °C | 478 - 484 J/(kg·K) Show Material materials with Calor específico of 478 - 484 J/(kg·K) | ||
400.0 °C | 490 - 495 J/(kg·K) Show Material materials with Calor específico of 490 - 495 J/(kg·K) | ||
500.0 °C | 523 J/(kg·K) Show Material materials with Calor específico of 523 J/(kg·K) | ||
600.0 °C | 544 J/(kg·K) Show Material materials with Calor específico of 544 J/(kg·K) | ||
700.0 °C | 555 J/(kg·K) Show Material materials with Calor específico of 555 J/(kg·K) | ||
800.0 °C | 566 J/(kg·K) Show Material materials with Calor específico of 566 J/(kg·K) | ||
900.0 °C | 577 J/(kg·K) Show Material materials with Calor específico of 577 J/(kg·K) | ||
1000.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
1150.0 °C | 603 J/(kg·K) Show Material materials with Calor específico of 603 J/(kg·K) | ||
Coeficiente de dilatación térmica | -130.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | |
-75.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
93.0 °C | 1.39E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.39E-5 1/K | ||
100.0 °C | 1.38E-5 - 1.39E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.38E-5 - 1.39E-5 1/K | ||
200.0 °C | 1.45E-5 - 1.55E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 - 1.55E-5 1/K | ||
300.0 °C | 1.49E-5 - 1.58E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 - 1.58E-5 1/K | ||
400.0 °C | 1.52E-5 - 1.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.52E-5 - 1.6E-5 1/K | ||
500.0 °C | 1.56E-5 - 1.63E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.56E-5 - 1.63E-5 1/K | ||
600.0 °C | 1.6E-5 - 1.66E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.66E-5 1/K | ||
700.0 °C | 1.64E-5 - 1.7E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.64E-5 - 1.7E-5 1/K | ||
800.0 °C | 1.68E-5 - 1.74E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.68E-5 - 1.74E-5 1/K | ||
900.0 °C | 1.73E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.73E-5 - 1.77E-5 1/K | ||
Conductividad térmica | -130.0 °C | 22 W/(m·K) Show Material materials with Conductividad térmica of 22 W/(m·K) | |
-75.0 °C | 24 W/(m·K) Show Material materials with Conductividad térmica of 24 W/(m·K) | ||
20.0 °C | 21.8 - 26 W/(m·K) Show Material materials with Conductividad térmica of 21.8 - 26 W/(m·K) | ||
100.0 °C | 25.4 - 29.5 W/(m·K) Show Material materials with Conductividad térmica of 25.4 - 29.5 W/(m·K) | ||
200.0 °C | 28.7 - 33 W/(m·K) Show Material materials with Conductividad térmica of 28.7 - 33 W/(m·K) | ||
300.0 °C | 31.9 - 36.5 W/(m·K) Show Material materials with Conductividad térmica of 31.9 - 36.5 W/(m·K) | ||
400.0 °C | 34.7 - 440 W/(m·K) Show Material materials with Conductividad térmica of 34.7 - 440 W/(m·K) | ||
500.0 °C | 38.4 - 44 W/(m·K) Show Material materials with Conductividad térmica of 38.4 - 44 W/(m·K) | ||
600.0 °C | 41.2 - 48.5 W/(m·K) Show Material materials with Conductividad térmica of 41.2 - 48.5 W/(m·K) | ||
700.0 °C | 43.1 - 52 W/(m·K) Show Material materials with Conductividad térmica of 43.1 - 52 W/(m·K) | ||
800.0 °C | 45.1 - 56 W/(m·K) Show Material materials with Conductividad térmica of 45.1 - 56 W/(m·K) | ||
900.0 °C | 47.5 - 58 W/(m·K) Show Material materials with Conductividad térmica of 47.5 - 58 W/(m·K) | ||
1000.0 °C | 50 W/(m·K) Show Material materials with Conductividad térmica of 50 W/(m·K) | ||
1150.0 °C | 52.9 W/(m·K) Show Material materials with Conductividad térmica of 52.9 W/(m·K) | ||
Temperatura de fusión | 1170 - 1365 °C Show Material materials with Temperatura de fusión of 1170 - 1365 °C | Typical for Nickel Copper Alloy | |
Temperatura máx. de funcionamiento, largo | -10 - 450 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -10 - 450 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 5.13E-7 - 5.47E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.13E-7 - 5.47E-7 Ω·m |
100.0 °C | 5.4E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.4E-7 Ω·m | |
200.0 °C | 5.55E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.55E-7 Ω·m | |
300.0 °C | 5.75E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.75E-7 Ω·m | |
400.0 °C | 5.85E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.85E-7 Ω·m | |
500.0 °C | 6E-7 Ω·m Show Material materials with Resistividad eléctrica of 6E-7 Ω·m | |
600.0 °C | 6.18E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.18E-7 Ω·m | |
700.0 °C | 6.35E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.35E-7 Ω·m | |
800.0 °C | 6.55E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.55E-7 Ω·m | |
900.0 °C | 6.75E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.75E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.5 % Show Material materials with Aluminio of 0.5 % |
Azufre | 0.02 - 0.024 % Show Material materials with Azufre of 0.02 - 0.024 % |
Carbono | 0.15 - 0.3 % Show Material materials with Carbono of 0.15 - 0.3 % |
Cobalto | 2 % Show Material materials with Cobalto of 2 % |
Cobre | 28 - 34 % Show Material materials with Cobre of 28 - 34 % |
Hierro | 1 - 2.5 % Show Material materials with Hierro of 1 - 2.5 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Níquel | 63 % Show Material materials with Níquel of 63 % |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % |
Titanio | 0.3 % Show Material materials with Titanio of 0.3 % |