General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20.0 °C | 4.505 g/cm³ Show Material materials with Densidad of 4.505 g/cm³ | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dureza Brinell | 20.0 °C | 170.0 Show Material materials with Dureza Brinell of 170.0 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | |
Elongación | 20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | Annealed | DIN 17851, DIN 17864, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17860 | Welded Tube | ||
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
Estricción | 20.0 °C | 30.0 % Show Material materials with Estricción of 30.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 30.0 % Show Material materials with Estricción of 30.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
Módulo de cizallamiento | 20.0 °C | 45.0 GPa Show Material materials with Módulo de cizallamiento of 45.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | |
Módulo elástico | 20.0 °C | 108.0 - 110.0 GPa Show Material materials with Módulo elástico of 108.0 - 110.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube | |
20.0 °C | 108.0 GPa Show Material materials with Módulo elástico of 108.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | ||
200.0 °C | 96.0 - 97.0 GPa Show Material materials with Módulo elástico of 96.0 - 97.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube | ||
200.0 °C | 96.0 GPa Show Material materials with Módulo elástico of 96.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | ||
400.0 °C | 82.0 GPa Show Material materials with Módulo elástico of 82.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
Resistencia a la tracción | 20.0 °C | 460.0 - 590.0 MPa Show Material materials with Resistencia a la tracción of 460.0 - 590.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Welded Tube | |
20.0 °C | 460.0 - 590.0 MPa Show Material materials with Resistencia a la tracción of 460.0 - 590.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse | |
20.0 °C | 560.0 MPa Show Material materials with Resistencia a la tracción of 560.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
100.0 °C | 460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
200.0 °C | 340.0 MPa Show Material materials with Resistencia a la tracción of 340.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
300.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 520.0 J/(kg·K) Show Material materials with Calor específico of 520.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | |
200.0 °C | 570.0 J/(kg·K) Show Material materials with Calor específico of 570.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
400.0 °C | 630.0 J/(kg·K) Show Material materials with Calor específico of 630.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
Coeficiente de dilatación térmica | 200.0 °C | 9.1e-06 1/K Show Material materials with Coeficiente de dilatación térmica of 9.1e-06 1/K | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | |
400.0 °C | 9.2e-06 1/K Show Material materials with Coeficiente de dilatación térmica of 9.2e-06 1/K | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | ||
Conductividad térmica | 20.0 °C | 22.6 W/(m·K) Show Material materials with Conductividad térmica of 22.6 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | |
200.0 °C | 20.9 W/(m·K) Show Material materials with Conductividad térmica of 20.9 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
400.0 °C | 19.3 W/(m·K) Show Material materials with Conductividad térmica of 19.3 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
Temperatura de fusión | 1540.0 - 1715.0 °C Show Material materials with Temperatura de fusión of 1540.0 - 1715.0 °C | Typical for Titanium Near Alpha Alloy |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Resistividad eléctrica | 20.0 °C | 5.2e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.2e-07 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
200.0 °C | 8.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.7e-07 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | |
400.0 °C | 1.2e-06 Ω·m Show Material materials with Resistividad eléctrica of 1.2e-06 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbono | 0.06 Show Material materials with Carbono of 0.06 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Hidrógeno | 0.013 Show Material materials with Hidrógeno of 0.013 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Hierro | 0.25 Show Material materials with Hierro of 0.25 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Nitrógeno | 0.05 Show Material materials with Nitrógeno of 0.05 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Oxígeno | 0.25 Show Material materials with Oxígeno of 0.25 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Paladio | 0.15 - 0.25 % Show Material materials with Paladio of 0.15 - 0.25 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Titanio | 98.7 % Show Material materials with Titanio of 98.7 % | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Tube, Forging, Rod, Welded Tube |