General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel |
Módulo de cizallamiento | 23.0 °C | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | ||
100.0 °C | 207 - 208 GPa Show Material materials with Módulo elástico of 207 - 208 GPa | ||
200.0 °C | 199 - 201 GPa Show Material materials with Módulo elástico of 199 - 201 GPa | ||
300.0 °C | 192 - 193 GPa Show Material materials with Módulo elástico of 192 - 193 GPa | ||
400.0 °C | 184 - 185 GPa Show Material materials with Módulo elástico of 184 - 185 GPa | ||
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 - 500 J/(kg·K) Show Material materials with Calor específico of 479 - 500 J/(kg·K) | ||
200.0 °C | 499 - 540 J/(kg·K) Show Material materials with Calor específico of 499 - 540 J/(kg·K) | ||
300.0 °C | 517 - 580 J/(kg·K) Show Material materials with Calor específico of 517 - 580 J/(kg·K) | ||
400.0 °C | 536 - 620 J/(kg·K) Show Material materials with Calor específico of 536 - 620 J/(kg·K) | ||
500.0 °C | 558 - 690 J/(kg·K) Show Material materials with Calor específico of 558 - 690 J/(kg·K) | ||
600.0 °C | 587 - 780 J/(kg·K) Show Material materials with Calor específico of 587 - 780 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
100.0 °C | 1.22E-5 - 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22E-5 - 1.25E-5 1/K | ||
200.0 °C | 1.29E-5 - 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29E-5 - 1.3E-5 1/K | ||
300.0 °C | 1.34E-5 - 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.34E-5 - 1.36E-5 1/K | ||
400.0 °C | 1.4E-5 - 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 - 1.41E-5 1/K | ||
500.0 °C | 1.43E-5 - 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.43E-5 - 1.45E-5 1/K | ||
600.0 °C | 1.46E-5 - 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.46E-5 - 1.49E-5 1/K | ||
Conductividad térmica | 20.0 °C | 46.5 W/(m·K) Show Material materials with Conductividad térmica of 46.5 W/(m·K) | |
100.0 °C | 47 - 47.2 W/(m·K) Show Material materials with Conductividad térmica of 47 - 47.2 W/(m·K) | ||
200.0 °C | 45.9 - 46 W/(m·K) Show Material materials with Conductividad térmica of 45.9 - 46 W/(m·K) | ||
300.0 °C | 43.5 - 44 W/(m·K) Show Material materials with Conductividad térmica of 43.5 - 44 W/(m·K) | ||
400.0 °C | 40.9 - 41 W/(m·K) Show Material materials with Conductividad térmica of 40.9 - 41 W/(m·K) | ||
500.0 °C | 38 - 38.1 W/(m·K) Show Material materials with Conductividad térmica of 38 - 38.1 W/(m·K) | ||
600.0 °C | 35 - 35.3 W/(m·K) Show Material materials with Conductividad térmica of 35 - 35.3 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | |
100.0 °C | 12.2 mm²/s Show Material materials with Difusividad térmica of 12.2 mm²/s | ||
200.0 °C | 11.1 mm²/s Show Material materials with Difusividad térmica of 11.1 mm²/s | ||
300.0 °C | 9.9 mm²/s Show Material materials with Difusividad térmica of 9.9 mm²/s | ||
400.0 °C | 8.7 mm²/s Show Material materials with Difusividad térmica of 8.7 mm²/s | ||
500.0 °C | 7.3 mm²/s Show Material materials with Difusividad térmica of 7.3 mm²/s | ||
600.0 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 2.24E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.24E-7 Ω·m |
100.0 °C | 2.7E-7 - 2.71E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.7E-7 - 2.71E-7 Ω·m | |
200.0 °C | 3.4E-7 - 3.44E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.4E-7 - 3.44E-7 Ω·m | |
300.0 °C | 4.3E-7 - 4.31E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.3E-7 - 4.31E-7 Ω·m | |
400.0 °C | 5.3E-7 - 5.32E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.3E-7 - 5.32E-7 Ω·m | |
500.0 °C | 6.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.5E-7 Ω·m | |
600.0 °C | 7.86E-7 - 7.9E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.86E-7 - 7.9E-7 Ω·m | |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.02 - 0.05 % Show Material materials with Aluminio of 0.02 - 0.05 % |
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % |
Carbono | 0.12 - 0.18 % Show Material materials with Carbono of 0.12 - 0.18 % |
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 0.7 - 0.9 % Show Material materials with Manganeso of 0.7 - 0.9 % |
Silicona | 0.2 % Show Material materials with Silicona of 0.2 % |