General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.82 - 7.85 g/cm³ Show Material materials with Densidad of 7.82 - 7.85 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Chromium Steel |
Módulo de cizallamiento | 20.0 °C | 81 GPa Show Material materials with Módulo de cizallamiento of 81 GPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | |
20.0 °C | 210 - 212 GPa Show Material materials with Módulo elástico of 210 - 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | ||
200.0 °C | 195 - 199 GPa Show Material materials with Módulo elástico of 195 - 199 GPa | ||
300.0 °C | 185 - 192 GPa Show Material materials with Módulo elástico of 185 - 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 460 - 461 J/(kg·K) Show Material materials with Calor específico of 460 - 461 J/(kg·K) | ||
100.0 °C | 479 - 480 J/(kg·K) Show Material materials with Calor específico of 479 - 480 J/(kg·K) | ||
200.0 °C | 499 - 520 J/(kg·K) Show Material materials with Calor específico of 499 - 520 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
100.0 °C | 1.1E-5 - 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 - 1.25E-5 1/K | ||
200.0 °C | 1.12E-5 - 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.12E-5 - 1.3E-5 1/K | ||
300.0 °C | 1.25E-5 - 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 - 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | ||
Conductividad térmica | 20.0 °C | 39.6 - 44 W/(m·K) Show Material materials with Conductividad térmica of 39.6 - 44 W/(m·K) | |
100.0 °C | 41 - 41.9 W/(m·K) Show Material materials with Conductividad térmica of 41 - 41.9 W/(m·K) | ||
200.0 °C | 39.8 - 41 W/(m·K) Show Material materials with Conductividad térmica of 39.8 - 41 W/(m·K) | ||
300.0 °C | 39.9 W/(m·K) Show Material materials with Conductividad térmica of 39.9 W/(m·K) | ||
400.0 °C | 38.1 W/(m·K) Show Material materials with Conductividad térmica of 38.1 W/(m·K) | ||
500.0 °C | 35.9 W/(m·K) Show Material materials with Conductividad térmica of 35.9 W/(m·K) | ||
600.0 °C | 33.6 W/(m·K) Show Material materials with Conductividad térmica of 33.6 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 11 mm²/s Show Material materials with Difusividad térmica of 11 mm²/s | |
100.0 °C | 10.6 mm²/s Show Material materials with Difusividad térmica of 10.6 mm²/s | ||
200.0 °C | 9.9 mm²/s Show Material materials with Difusividad térmica of 9.9 mm²/s | ||
300.0 °C | 9 mm²/s Show Material materials with Difusividad térmica of 9 mm²/s | ||
400.0 °C | 8.1 mm²/s Show Material materials with Difusividad térmica of 8.1 mm²/s | ||
500.0 °C | 6.9 mm²/s Show Material materials with Difusividad térmica of 6.9 mm²/s | ||
600.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Steel | |
Temperatura máx. de funcionamiento, largo | -25 - 0 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -25 - 0 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.6E-7 - 2.63E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.6E-7 - 2.63E-7 Ω·m |
100.0 °C | 3.12E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.12E-7 Ω·m | |
200.0 °C | 3.85E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.85E-7 Ω·m | |
300.0 °C | 4.7E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.7E-7 Ω·m | |
400.0 °C | 5.71E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.71E-7 Ω·m | |
500.0 °C | 6.88E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.88E-7 Ω·m | |
600.0 °C | 8.25E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.25E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % |
Carbono | 0.14 - 0.2 % Show Material materials with Carbono of 0.14 - 0.2 % |
Cromo | 0.6 - 0.9 % Show Material materials with Cromo of 0.6 - 0.9 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 0.4 - 0.7 % Show Material materials with Manganeso of 0.4 - 0.7 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |