General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Densidad of 7.8 - 7.9 g/cm³ | Typical for Chromium Vanadium Steel |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Chromium Vanadium Steel |
Estricción | 20.0 °C | 40 - 50 % Show Material materials with Estricción of 40 - 50 % | |
Módulo de cizallamiento | 20.0 °C | 79.5 GPa Show Material materials with Módulo de cizallamiento of 79.5 GPa | |
Módulo elástico | 20.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa | |
Resistencia a la tracción | 20.0 °C | 1390 - 2060 MPa Show Material materials with Resistencia a la tracción of 1390 - 2060 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 1.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2E-5 1/K | Typical for Chromium Vanadium Steel |
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Vanadium Steel | |
Temperatura máx. de funcionamiento, largo | -60 - 200 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -60 - 200 °C |
Chemical properties
Property | Value |
---|---|
Azufre | 0.02 % Show Material materials with Azufre of 0.02 % |
Carbono | 0.62 - 0.72 % Show Material materials with Carbono of 0.62 - 0.72 % |
Cobre | 0.06 % Show Material materials with Cobre of 0.06 % |
Cromo | 0.4 - 0.6 % Show Material materials with Cromo of 0.4 - 0.6 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.5 - 0.9 % Show Material materials with Manganeso of 0.5 - 0.9 % |
Silicona | 0.15 - 0.3 % Show Material materials with Silicona of 0.15 - 0.3 % |
Vanadio | 0.15 - 0.25 % Show Material materials with Vanadio of 0.15 - 0.25 % |
Technological properties
Property | ||
---|---|---|
Features | Spring |