General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.12 g/cm³ Show Material materials with Densidad of 8.12 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
Módulo de cizallamiento | 23.0 °C | 79 GPa Show Material materials with Módulo de cizallamiento of 79 GPa | Typical for Tool And Machining Steel |
Módulo elástico | 20.0 °C | 224 GPa Show Material materials with Módulo elástico of 224 GPa | |
100.0 °C | 220 GPa Show Material materials with Módulo elástico of 220 GPa | ||
200.0 °C | 214 GPa Show Material materials with Módulo elástico of 214 GPa | ||
300.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | ||
400.0 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | ||
500.0 °C | 191 GPa Show Material materials with Módulo elástico of 191 GPa | ||
600.0 °C | 180 GPa Show Material materials with Módulo elástico of 180 GPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 420 - 460 J/(kg·K) Show Material materials with Calor específico of 420 - 460 J/(kg·K) | Typical for Tool And Machining Steel |
Coeficiente de dilatación térmica | -100.0 °C | 9.6E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 9.6E-6 1/K | |
20.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | ||
100.0 °C | 1.11E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.11E-5 1/K | ||
200.0 °C | 1.16E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.16E-5 1/K | ||
300.0 °C | 1.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2E-5 1/K | ||
400.0 °C | 1.24E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.24E-5 1/K | ||
500.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
600.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | ||
Conductividad térmica | 20.0 °C | 27.6 W/(m·K) Show Material materials with Conductividad térmica of 27.6 W/(m·K) | |
100.0 °C | 27.9 W/(m·K) Show Material materials with Conductividad térmica of 27.9 W/(m·K) | ||
200.0 °C | 27.7 W/(m·K) Show Material materials with Conductividad térmica of 27.7 W/(m·K) | ||
300.0 °C | 27.5 W/(m·K) Show Material materials with Conductividad térmica of 27.5 W/(m·K) | ||
400.0 °C | 27 W/(m·K) Show Material materials with Conductividad térmica of 27 W/(m·K) | ||
500.0 °C | 26.6 W/(m·K) Show Material materials with Conductividad térmica of 26.6 W/(m·K) | ||
600.0 °C | 26.1 W/(m·K) Show Material materials with Conductividad térmica of 26.1 W/(m·K) | ||
Temperatura de fusión | 1370 - 1425 °C Show Material materials with Temperatura de fusión of 1370 - 1425 °C | Typical for Tool And Machining Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 5.24E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.24E-7 Ω·m |
100.0 °C | 5.81E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.81E-7 Ω·m | |
200.0 °C | 6.64E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.64E-7 Ω·m | |
300.0 °C | 7.51E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.51E-7 Ω·m | |
400.0 °C | 8.44E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.44E-7 Ω·m | |
500.0 °C | 9.41E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.41E-7 Ω·m | |
600.0 °C | 1.04E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.04E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % |
Carbono | 1.2 - 1.35 % Show Material materials with Carbono of 1.2 - 1.35 % |
Cobalto | 9.5 - 10.5 % Show Material materials with Cobalto of 9.5 - 10.5 % |
Cromo | 3.8 - 4.5 % Show Material materials with Cromo of 3.8 - 4.5 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.4 % Show Material materials with Manganeso of 0.4 % |
Molibdeno | 3.2 - 3.9 % Show Material materials with Molibdeno of 3.2 - 3.9 % |
Silicona | 0.45 % Show Material materials with Silicona of 0.45 % |
Vanadio | 3 - 3.5 % Show Material materials with Vanadio of 3 - 3.5 % |
Wolframio | 9 - 10 % Show Material materials with Wolframio of 9 - 10 % |