General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.68 g/cm³ Show Material materials with Densidad of 7.68 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Tool And Machining Steel |
Módulo de cizallamiento | 23.0 °C | 79 GPa Show Material materials with Módulo de cizallamiento of 79 GPa | Typical for Tool And Machining Steel |
Módulo elástico | 20.0 °C | 215 GPa Show Material materials with Módulo elástico of 215 GPa | |
100.0 °C | 211 GPa Show Material materials with Módulo elástico of 211 GPa | ||
200.0 °C | 204 GPa Show Material materials with Módulo elástico of 204 GPa | ||
300.0 °C | 198 GPa Show Material materials with Módulo elástico of 198 GPa | ||
400.0 °C | 191 GPa Show Material materials with Módulo elástico of 191 GPa | ||
500.0 °C | 182 GPa Show Material materials with Módulo elástico of 182 GPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 439 J/(kg·K) Show Material materials with Calor específico of 439 J/(kg·K) | |
Coeficiente de dilatación térmica | -100.0 °C | 8.6E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 8.6E-6 1/K | |
20.0 °C | 1.01E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.01E-5 1/K | ||
100.0 °C | 1.07E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.07E-5 1/K | ||
200.0 °C | 1.13E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.13E-5 1/K | ||
300.0 °C | 1.18E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.18E-5 1/K | ||
400.0 °C | 1.22E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22E-5 1/K | ||
500.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | ||
Conductividad térmica | 20.0 °C | 31.9 W/(m·K) Show Material materials with Conductividad térmica of 31.9 W/(m·K) | |
100.0 °C | 31.5 W/(m·K) Show Material materials with Conductividad térmica of 31.5 W/(m·K) | ||
200.0 °C | 30.9 W/(m·K) Show Material materials with Conductividad térmica of 30.9 W/(m·K) | ||
300.0 °C | 29.7 W/(m·K) Show Material materials with Conductividad térmica of 29.7 W/(m·K) | ||
400.0 °C | 28.6 W/(m·K) Show Material materials with Conductividad térmica of 28.6 W/(m·K) | ||
500.0 °C | 27.6 W/(m·K) Show Material materials with Conductividad térmica of 27.6 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 9.5 mm²/s Show Material materials with Difusividad térmica of 9.5 mm²/s | |
Temperatura de fusión | 1370 - 1425 °C Show Material materials with Temperatura de fusión of 1370 - 1425 °C | Typical for Tool And Machining Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 4.53E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.53E-7 Ω·m |
100.0 °C | 5.15E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.15E-7 Ω·m | |
200.0 °C | 5.96E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.96E-7 Ω·m | |
300.0 °C | 6.95E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.95E-7 Ω·m | |
400.0 °C | 7.98E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.98E-7 Ω·m | |
500.0 °C | 9.08E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.08E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % |
Carbono | 1.5 - 1.6 % Show Material materials with Carbono of 1.5 - 1.6 % |
Cromo | 11 - 12 % Show Material materials with Cromo of 11 - 12 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.15 - 0.45 % Show Material materials with Manganeso of 0.15 - 0.45 % |
Molibdeno | 0.6 - 0.8 % Show Material materials with Molibdeno of 0.6 - 0.8 % |
Silicona | 0.1 - 0.4 % Show Material materials with Silicona of 0.1 - 0.4 % |
Vanadio | 0.9 - 1.1 % Show Material materials with Vanadio of 0.9 - 1.1 % |