General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.74 g/cm³ Show Material materials with Densidad of 7.74 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
Módulo de cizallamiento | 23.0 °C | 79 GPa Show Material materials with Módulo de cizallamiento of 79 GPa | Typical for Tool And Machining Steel |
Módulo elástico | 20.0 °C | 210 GPa Show Material materials with Módulo elástico of 210 GPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-5 1/K | |
20.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | ||
100.0 °C | 1.13E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.13E-5 1/K | ||
200.0 °C | 1.18E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.18E-5 1/K | ||
300.0 °C | 1.23E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.23E-5 1/K | ||
400.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
500.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | ||
600.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ||
Conductividad térmica | 20.0 °C | 19.2 W/(m·K) Show Material materials with Conductividad térmica of 19.2 W/(m·K) | |
100.0 °C | 20.1 W/(m·K) Show Material materials with Conductividad térmica of 20.1 W/(m·K) | ||
200.0 °C | 22.4 W/(m·K) Show Material materials with Conductividad térmica of 22.4 W/(m·K) | ||
300.0 °C | 24 W/(m·K) Show Material materials with Conductividad térmica of 24 W/(m·K) | ||
400.0 °C | 25.1 W/(m·K) Show Material materials with Conductividad térmica of 25.1 W/(m·K) | ||
500.0 °C | 25.8 W/(m·K) Show Material materials with Conductividad térmica of 25.8 W/(m·K) | ||
600.0 °C | 26.1 W/(m·K) Show Material materials with Conductividad térmica of 26.1 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | |
100.0 °C | 5.3 mm²/s Show Material materials with Difusividad térmica of 5.3 mm²/s | ||
200.0 °C | 5.5 mm²/s Show Material materials with Difusividad térmica of 5.5 mm²/s | ||
300.0 °C | 5.5 mm²/s Show Material materials with Difusividad térmica of 5.5 mm²/s | ||
400.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
500.0 °C | 5 mm²/s Show Material materials with Difusividad térmica of 5 mm²/s | ||
600.0 °C | 4.4 mm²/s Show Material materials with Difusividad térmica of 4.4 mm²/s | ||
Temperatura de fusión | 1370 - 1425 °C Show Material materials with Temperatura de fusión of 1370 - 1425 °C | Typical for Tool And Machining Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 5.43E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.43E-7 Ω·m |
100.0 °C | 6.38E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.38E-7 Ω·m | |
200.0 °C | 7.05E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.05E-7 Ω·m | |
300.0 °C | 7.82E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.82E-7 Ω·m | |
400.0 °C | 8.68E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.68E-7 Ω·m | |
500.0 °C | 9.6E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.6E-7 Ω·m | |
600.0 °C | 1.06E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.06E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % |
Carbono | 0.36 - 0.42 % Show Material materials with Carbono of 0.36 - 0.42 % |
Cromo | 4.8 - 5.5 % Show Material materials with Cromo of 4.8 - 5.5 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.3 - 0.5 % Show Material materials with Manganeso of 0.3 - 0.5 % |
Molibdeno | 1.1 - 1.4 % Show Material materials with Molibdeno of 1.1 - 1.4 % |
Silicona | 0.9 - 1.2 % Show Material materials with Silicona of 0.9 - 1.2 % |
Vanadio | 0.25 - 0.5 % Show Material materials with Vanadio of 0.25 - 0.5 % |