General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.9 g/cm³ Show Material materials with Densidad of 7.9 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel |
Dureza Brinell | 20.0 °C | 200 [-] Show Material materials with Dureza Brinell of 200 [-] | |
Elongación | 20.0 °C | 30 % Show Material materials with Elongación of 30 % | |
Límite elástico Rp 0,2 | 20.0 °C | 235 MPa Show Material materials with Límite elástico Rp 0,2 of 235 MPa | |
Módulo elástico | 23.0 °C | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel |
Resistencia a la tracción | 20.0 °C | 490 - 740 MPa Show Material materials with Resistencia a la tracción of 490 - 740 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 20.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) |
Coeficiente de dilatación térmica | 400.0 °C | 1.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 1/K |
800.0 °C | 1.75E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 1/K | |
1000.0 °C | 1.85E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.85E-5 1/K | |
Conductividad térmica | 20.0 °C | 12 W/(m·K) Show Material materials with Conductividad térmica of 12 W/(m·K) |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.04E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.04E-6 Ω·m |
Chemical properties
Property | Value |
---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % |
Carbono | 0.12 % Show Material materials with Carbono of 0.12 % |
Cromo | 19 - 22 % Show Material materials with Cromo of 19 - 22 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 1.5 % Show Material materials with Manganeso of 1.5 % |
Níquel | 30 - 34 % Show Material materials with Níquel of 30 - 34 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |