General
Property | Value | Comment |
---|---|---|
Carbon equivalent (CET) | 0.38 [-] Show Material materials with Carbon equivalent (CET) of 0.38 [-] | max. for t ≤ 50 mm plate thickness |
0.4 [-] Show Material materials with Carbon equivalent (CET) of 0.4 [-] | max. for 50 < t ≤ 100 mm plate thickness | |
Densidad | 7.8 - 7.9 g/cm³ Show Material materials with Densidad of 7.8 - 7.9 g/cm³ | typical for low carbon steel |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Charpy impact energy, V-notch | -40 °C | 34 J Show Material materials with Charpy impact energy, V-notch of 34 J | for t ≤ 50 mm plate thickness | average |
-40 °C | 41 J Show Material materials with Charpy impact energy, V-notch of 41 J | for 50 < t ≤ 70 mm plate thickness | average | |
-40 °C | 50 J Show Material materials with Charpy impact energy, V-notch of 50 J | for 70 < t ≤ 100 mm plate thickness | average | |
Charpy impact energy, V-notch, transverse | -40 °C | 24 J Show Material materials with Charpy impact energy, V-notch, transverse of 24 J | for t ≤ 50 mm plate thickness | average |
-40 °C | 27 J Show Material materials with Charpy impact energy, V-notch, transverse of 27 J | for 50 < t ≤ 70 mm plate thickness | average | |
-40 °C | 34 J Show Material materials with Charpy impact energy, V-notch, transverse of 34 J | for 70 < t ≤ 100 mm plate thickness | average | |
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | typical for low carbon steel | |
Elongación | 21 % Show Material materials with Elongación of 21 % | min. | |
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | typical for low carbon steel | |
Módulo elástico | 200 - 215 GPa Show Material materials with Módulo elástico of 200 - 215 GPa | typical for low carbon steel | |
Resistencia a la tracción | 490 - 620 MPa Show Material materials with Resistencia a la tracción of 490 - 620 MPa |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 465 J/(kg·K) Show Material materials with Calor específico of 465 J/(kg·K) | typical for low carbon steel |
Coeficiente de dilatación térmica | 1.32e-05 - 1.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 - 1.38e-05 1/K | typical for low carbon steel |
Conductividad térmica | 25 - 93 W/(m·K) Show Material materials with Conductividad térmica of 25 - 93 W/(m·K) | typical for low carbon steel |
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | typical for low carbon steel |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | typical for carbon steel |
Eléctrico
Property | Value | Comment |
---|---|---|
Resistividad eléctrica | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.43e-07 - 1.74e-07 Ω·m | typical for carbon steel |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminio | 0.015 % Show Material materials with Aluminio of 0.015 % | min. |
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % | max. |
Calcio | 0.005 % Show Material materials with Calcio of 0.005 % | max. |
Carbono | 0.18 % Show Material materials with Carbono of 0.18 % | max. |
Cobre | 0.35 % Show Material materials with Cobre of 0.35 % | max. |
Cromo | 0.2 % Show Material materials with Cromo of 0.2 % | max. |
Fósforo | 0.035 % Show Material materials with Fósforo of 0.035 % | max. |
Manganeso | 0.9 - 1.6 % Show Material materials with Manganeso of 0.9 - 1.6 % | |
Molibdeno | 0.08 % Show Material materials with Molibdeno of 0.08 % | max. |
Niobio | 0.02 - 0.05 % Show Material materials with Niobio of 0.02 - 0.05 % | |
Níquel | 0.4 % Show Material materials with Níquel of 0.4 % | max. |
Silicona | 0.1 - 0.5 % Show Material materials with Silicona of 0.1 - 0.5 % | |
Titanio | 0.02 % Show Material materials with Titanio of 0.02 % | max. |
Vanadio | 0.05 - 0.1 % Show Material materials with Vanadio of 0.05 - 0.1 % |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |