General
Property | Value | Comment |
---|---|---|
Carbon equivalent (CEV) | 0.43 [-] Show Material materials with Carbon equivalent (CEV) of 0.43 [-] | for t ≤ 50 mm plate thickness condition TM |
0.44 [-] Show Material materials with Carbon equivalent (CEV) of 0.44 [-] | for t ≤ 50 mm sections condition TM | |
0.45 [-] Show Material materials with Carbon equivalent (CEV) of 0.45 [-] | for 50 < t ≤100 mm plate thickness condition TM | |
0.45 [-] Show Material materials with Carbon equivalent (CEV) of 0.45 [-] | for t ≤ 50 mm plate thickness condition QT | |
0.46 [-] Show Material materials with Carbon equivalent (CEV) of 0.46 [-] | for t ≤ 50 mm plate thickness condition N/NR | |
0.47 [-] Show Material materials with Carbon equivalent (CEV) of 0.47 [-] | for t ≤ 50 mm sections condition N/NR | |
0.47 [-] Show Material materials with Carbon equivalent (CEV) of 0.47 [-] | for t ≤ 65 mm tabulars condition N/NR | |
0.47 [-] Show Material materials with Carbon equivalent (CEV) of 0.47 [-] | for 100 < t ≤ 250 mm plate thickness condition TM | |
0.47 [-] Show Material materials with Carbon equivalent (CEV) of 0.47 [-] | for 50 < t ≤100 mm plate thickness condition QT | |
0.48 [-] Show Material materials with Carbon equivalent (CEV) of 0.48 [-] | for 50 < t ≤100 mm plate thickness condition N/NR | |
0.49 [-] Show Material materials with Carbon equivalent (CEV) of 0.49 [-] | for 100 < t ≤ 250 mm plate thickness condition QT | |
0.52 [-] Show Material materials with Carbon equivalent (CEV) of 0.52 [-] | for 100 < t ≤ 250 mm plate thickness condition N/NR | |
0.53 [-] Show Material materials with Carbon equivalent (CEV) of 0.53 [-] | for t ≤ 250 or d ≤ 250 mm bars condition N/NR | |
Densidad | 7.8 - 7.9 g/cm³ Show Material materials with Densidad of 7.8 - 7.9 g/cm³ | typical for low carbon steel |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Charpy impact energy, V-notch | -20 °C | 41 J Show Material materials with Charpy impact energy, V-notch of 41 J | |
Charpy impact energy, V-notch, transverse | -20 °C | 27 J Show Material materials with Charpy impact energy, V-notch, transverse of 27 J | |
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | typical for low carbon steel | |
Elongación | 18 % Show Material materials with Elongación of 18 % | min. | |
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | typical for low carbon steel | |
Módulo elástico | 200 - 215 GPa Show Material materials with Módulo elástico of 200 - 215 GPa | typical for low carbon steel | |
Resistencia a la tracción | 530 - 680 MPa Show Material materials with Resistencia a la tracción of 530 - 680 MPa |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 465 J/(kg·K) Show Material materials with Calor específico of 465 J/(kg·K) | typical for low carbon steel |
Coeficiente de dilatación térmica | 1.32e-05 - 1.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 - 1.38e-05 1/K | typical for low carbon steel |
Conductividad térmica | 25 - 93 W/(m·K) Show Material materials with Conductividad térmica of 25 - 93 W/(m·K) | typical for low carbon steel |
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | typical for low carbon steel |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | typical for carbon steel |
Eléctrico
Property | Value | Comment |
---|---|---|
Resistividad eléctrica | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.43e-07 - 1.74e-07 Ω·m | typical for carbon steel |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminio | 0.018 - 0.2 % Show Material materials with Aluminio of 0.018 - 0.2 % | min., depending on the delivery condition |
Azufre | 0.01 - 0.025 % Show Material materials with Azufre of 0.01 - 0.025 % | max., depending on the delivery condition |
Boro | 0.005 % Show Material materials with Boro of 0.005 % | max. |
Calcio | 0.005 % Show Material materials with Calcio of 0.005 % | max. |
Carbono | 0.16 - 0.2 % Show Material materials with Carbono of 0.16 - 0.2 % | max., depending on the delivery condition |
Cobre | 0.5 - 0.55 % Show Material materials with Cobre of 0.5 - 0.55 % | max., depending on the delivery condition |
Cromo | 0.3 - 2 % Show Material materials with Cromo of 0.3 - 2 % | max., depending on the delivery condition |
Fósforo | 0.025 - 0.03 % Show Material materials with Fósforo of 0.025 - 0.03 % | max., depending on the delivery condition |
Manganeso | 1 - 1.7 % Show Material materials with Manganeso of 1 - 1.7 % | depending on the delivery condition |
Molibdeno | 0.1 - 0.7 % Show Material materials with Molibdeno of 0.1 - 0.7 % | max., depending on the delivery condition |
Niobio | 0.05 - 0.06 % Show Material materials with Niobio of 0.05 - 0.06 % | max., depending on the delivery condition |
Nitrógeno | 0.015 - 0.025 % Show Material materials with Nitrógeno of 0.015 - 0.025 % | max., depending on the delivery condition |
Níquel | 0.8 - 3.5 % Show Material materials with Níquel of 0.8 - 3.5 % | max., depending on the delivery condition |
Silicona | 0.6 - 0.8 % Show Material materials with Silicona of 0.6 - 0.8 % | max., depending on the delivery condition |
Titanio | 0.05 % Show Material materials with Titanio of 0.05 % | max. |
Vanadio | 0.12 - 0.2 % Show Material materials with Vanadio of 0.12 - 0.2 % | max., depending on the delivery condition |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |