General
Property | Value | Comment |
---|---|---|
Carbon equivalent (CET) | 0.4 [-] Show Material materials with Carbon equivalent (CET) of 0.4 [-] | |
Carbon equivalent (CEV) | 0.64 [-] Show Material materials with Carbon equivalent (CEV) of 0.64 [-] | for t ≤ 50 mm plate thickness |
0.66 [-] Show Material materials with Carbon equivalent (CEV) of 0.66 [-] | for 50 < t ≤100 mm plate thickness | |
0.68 [-] Show Material materials with Carbon equivalent (CEV) of 0.68 [-] | t ≤ 65 mm tabulars | |
0.7 [-] Show Material materials with Carbon equivalent (CEV) of 0.7 [-] | for 100 < t ≤ 250 mm plate thickness | |
Densidad | 7.8 - 7.9 g/cm³ Show Material materials with Densidad of 7.8 - 7.9 g/cm³ | typical for low carbon steel |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Charpy impact energy, V-notch | -40 °C | 62 J Show Material materials with Charpy impact energy, V-notch of 62 J | min. |
Charpy impact energy, V-notch, transverse | -40 °C | 46 J Show Material materials with Charpy impact energy, V-notch, transverse of 46 J | min. |
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | typical for low carbon steel | |
Elongación | 14 % Show Material materials with Elongación of 14 % | min., Transverse | |
16 % Show Material materials with Elongación of 16 % | min. | ||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | typical for low carbon steel | |
Módulo elástico | 200 - 215 GPa Show Material materials with Módulo elástico of 200 - 215 GPa | typical for low carbon steel | |
Resistencia a la tracción | 770 - 940 MPa Show Material materials with Resistencia a la tracción of 770 - 940 MPa |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 465 J/(kg·K) Show Material materials with Calor específico of 465 J/(kg·K) | typical for low carbon steel |
Coeficiente de dilatación térmica | 1.32e-05 - 1.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 - 1.38e-05 1/K | typical for low carbon steel |
Conductividad térmica | 25 - 93 W/(m·K) Show Material materials with Conductividad térmica of 25 - 93 W/(m·K) | typical for low carbon steel |
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | typical for low carbon steel |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | typical for carbon steel |
Eléctrico
Property | Value | Comment |
---|---|---|
Resistividad eléctrica | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.43e-07 - 1.74e-07 Ω·m | typical for carbon steel |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminio | 0.018 % Show Material materials with Aluminio of 0.018 % | min. |
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | can be 0.005% higher than the specified value |
Carbono | 0.18 % Show Material materials with Carbono of 0.18 % | |
Cobre | 0.5 % Show Material materials with Cobre of 0.5 % | |
Cromo | 1.5 % Show Material materials with Cromo of 1.5 % | |
Fósforo | 0.015 % Show Material materials with Fósforo of 0.015 % | can be 0.005% higher than the specified value |
Manganeso | 1.7 % Show Material materials with Manganeso of 1.7 % | |
Molibdeno | 0.7 % Show Material materials with Molibdeno of 0.7 % | |
Niobio | 0.06 % Show Material materials with Niobio of 0.06 % | |
Nitrógeno | 0.015 % Show Material materials with Nitrógeno of 0.015 % | the total aluminium to nitrogen ratio shall be a minimum of 2:1. When other nitrogen binding elements are used, the minimum Al value and Al/N ratio do not apply |
Níquel | 2 % Show Material materials with Níquel of 2 % | higher Ni content may be qualified and accepted subject to qualification during manufacturer qualification testing |
Oxígeno | 0.003 % Show Material materials with Oxígeno of 0.003 % | |
Titanio | 0.05 % Show Material materials with Titanio of 0.05 % | |
Vanadio | 0.12 % Show Material materials with Vanadio of 0.12 % |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |