General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 8.95 g/cm³ Show Material materials with Densidad of 8.95 g/cm³ | Typical for Wrought Copper Nickel Grade |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación A50 | 23.0 °C | 30 % Show Material materials with Elongación A50 of 30 % | |
Límite elástico Rp0.5 | 23.0 °C | 124 - 138 MPa Show Material materials with Límite elástico Rp0.5 of 124 - 138 MPa | |
Módulo elástico | 23.0 °C | 120 - 156 GPa Show Material materials with Módulo elástico of 120 - 156 GPa | Typical for Wrought Copper Nickel Grade |
Resistencia a la tracción | 23.0 °C | 310 - 345 MPa Show Material materials with Resistencia a la tracción of 310 - 345 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 375 - 398 J/(kg·K) Show Material materials with Calor específico of 375 - 398 J/(kg·K) | Typical for Wrought Copper Nickel Grade |
Coeficiente de dilatación térmica | 23.0 °C | 1.4E-5 - 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 - 1.8E-5 1/K | Typical for Wrought Copper Nickel Grade |
Conductividad térmica | 23.0 °C | 21 - 195 W/(m·K) Show Material materials with Conductividad térmica of 21 - 195 W/(m·K) | Typical for Wrought Copper Nickel Grade |
Temperatura de fusión | 915 - 1240 °C Show Material materials with Temperatura de fusión of 915 - 1240 °C | Typical for Wrought Copper Nickel Grade |
Chemical properties
Property | Value |
---|---|
Azufre | 0.02 % Show Material materials with Azufre of 0.02 % |
Cobre | 65 % Show Material materials with Cobre of 65 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Hierro | 0.4 - 1 % Show Material materials with Hierro of 0.4 - 1 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Níquel | 29 - 33 % Show Material materials with Níquel of 29 - 33 % |
Plomo | 0.02 % Show Material materials with Plomo of 0.02 % |
Zinc | 0.5 % Show Material materials with Zinc of 0.5 % |