Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Rockwell B | 23.0 °C | 88 - 99 [-] Show Material materials with Dureza Rockwell B of 88 - 99 [-] | |
Elongación A50 | 23.0 °C | 12 % Show Material materials with Elongación A50 of 12 % | |
Hardness, Rockwell Superficial 30-T | 23.0 °C | 75 - 82 [-] Show Material materials with Hardness, Rockwell Superficial 30-T of 75 - 82 [-] | |
Límite elástico Rp 0,2 | 23.0 °C | 550 - 690 MPa Show Material materials with Límite elástico Rp 0,2 of 550 - 690 MPa | |
Módulo elástico | 23.0 °C | 110 - 130 GPa Show Material materials with Módulo elástico of 110 - 130 GPa | Typical for Wrought Copper High Copper Alloy |
Resistencia a la tracción | 23.0 °C | 655 - 790 MPa Show Material materials with Resistencia a la tracción of 655 - 790 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 360 - 420 J/(kg·K) Show Material materials with Calor específico of 360 - 420 J/(kg·K) | Typical for Wrought Copper High Copper Alloy |
Coeficiente de dilatación térmica | 23.0 °C | 1.6E-5 - 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.8E-5 1/K | Typical for Wrought Copper High Copper Alloy |
Temperatura de fusión | 855 - 1090 °C Show Material materials with Temperatura de fusión of 855 - 1090 °C | Typical for Wrought Copper High Copper Alloy |
Eléctrico
Property | Value |
---|---|
Specific Electrical conductivity | 50 % IACS Show Material materials with Specific Electrical conductivity of 50 % IACS |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.2 % Show Material materials with Aluminio of 0.2 % |
Berilio | 0.15 - 0.5 % Show Material materials with Berilio of 0.15 - 0.5 % |
Circonio | 0.5 % Show Material materials with Circonio of 0.5 % |
Estaño | 0.25 % Show Material materials with Estaño of 0.25 % |
Hierro | 0.2 % Show Material materials with Hierro of 0.2 % |
Níquel | 0.5 - 1 % Show Material materials with Níquel of 0.5 - 1 % |
Silicona | 0.2 % Show Material materials with Silicona of 0.2 % |