General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 7.2 - 7.34 g/cm³ Show Material materials with Densidad of 7.2 - 7.34 g/cm³ | Typical for Malleable Cast Iron |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.27 [-] Show Material materials with Coeficiente de Poisson of 0.27 [-] | Typical for Malleable Cast Iron |
Dureza Brinell | 23.0 °C | 269 - 302 [-] Show Material materials with Dureza Brinell of 269 - 302 [-] | |
Elongación | 23.0 °C | 1 % Show Material materials with Elongación of 1 % | |
Límite elástico | 23.0 °C | 586 MPa Show Material materials with Límite elástico of 586 MPa | |
Módulo de cizallamiento | 23.0 °C | 64 GPa Show Material materials with Módulo de cizallamiento of 64 GPa | Typical for Malleable Cast Iron |
Módulo elástico | 23.0 °C | 179 GPa Show Material materials with Módulo elástico of 179 GPa | |
Resistencia a la tracción | 23.0 °C | 724 MPa Show Material materials with Resistencia a la tracción of 724 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 460 - 527 J/(kg·K) Show Material materials with Calor específico of 460 - 527 J/(kg·K) | Typical for Malleable Cast Iron |
Coeficiente de dilatación térmica | 23.0 °C | 1E-5 - 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-5 - 1.4E-5 1/K | Typical for Malleable Cast Iron |
Conductividad térmica | 23.0 °C | 51 W/(m·K) Show Material materials with Conductividad térmica of 51 W/(m·K) | Typical for Malleable Cast Iron |
Temperatura de fusión | 1120 °C Show Material materials with Temperatura de fusión of 1120 °C | Typical for Cast Iron |
Chemical properties
Property | Value | Comment |
---|---|---|
Azufre | 0.02 - 0.2 % Show Material materials with Azufre of 0.02 - 0.2 % | |
Carbono | 2.2 - 2.9 % Show Material materials with Carbono of 2.2 - 2.9 % | |
Fósforo | 0.02 - 0.1 % Show Material materials with Fósforo of 0.02 - 0.1 % | |
Hierro | 93.6 - 96.71 % Show Material materials with Hierro of 93.6 - 96.71 % | balance |
Manganeso | 0.15 - 1.25 % Show Material materials with Manganeso of 0.15 - 1.25 % | |
Silicona | 0.9 - 1.9 % Show Material materials with Silicona of 0.9 - 1.9 % |
Technological properties
Property | ||
---|---|---|
Application areas | Where high strength and/or wear resistance are required. | |
Processing history | as agreed |