General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 20.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Densidad of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] |
Elongación | 20.0 °C | 21 % Show Material materials with Elongación of 21 % |
Elongación transversal | 20.0 °C | 19 % Show Material materials with Elongación transversal of 19 % |
Límite elástico | 20.0 °C | 255 - 275 MPa Show Material materials with Límite elástico of 255 - 275 MPa |
Límite elástico Rp 0,2 | 50.0 °C | 255 - 275 MPa Show Material materials with Límite elástico Rp 0,2 of 255 - 275 MPa |
200.0 °C | 200 - 215 MPa Show Material materials with Límite elástico Rp 0,2 of 200 - 215 MPa | |
250.0 °C | 180 - 195 MPa Show Material materials with Límite elástico Rp 0,2 of 180 - 195 MPa | |
300.0 °C | 155 - 165 MPa Show Material materials with Límite elástico Rp 0,2 of 155 - 165 MPa | |
Límite elástico transversal | 20.0 °C | 255 - 275 MPa Show Material materials with Límite elástico transversal of 255 - 275 MPa |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa |
20.0 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | |
100.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | |
200.0 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | |
300.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | |
400.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | |
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | |
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | |
Resistencia a la tracción | 20.0 °C | 420 - 550 MPa Show Material materials with Resistencia a la tracción of 420 - 550 MPa |
Resistencia a la tracción transversal | 20.0 °C | 420 - 550 MPa Show Material materials with Resistencia a la tracción transversal of 420 - 550 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | ||
Conductividad térmica | 20.0 °C | 53.4 W/(m·K) Show Material materials with Conductividad térmica of 53.4 W/(m·K) | |
100.0 °C | 52.9 W/(m·K) Show Material materials with Conductividad térmica of 52.9 W/(m·K) | ||
200.0 °C | 50.3 W/(m·K) Show Material materials with Conductividad térmica of 50.3 W/(m·K) | ||
300.0 °C | 46.7 W/(m·K) Show Material materials with Conductividad térmica of 46.7 W/(m·K) | ||
400.0 °C | 43.3 W/(m·K) Show Material materials with Conductividad térmica of 43.3 W/(m·K) | ||
500.0 °C | 39.8 W/(m·K) Show Material materials with Conductividad térmica of 39.8 W/(m·K) | ||
600.0 °C | 36.7 W/(m·K) Show Material materials with Conductividad térmica of 36.7 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 14.8 mm²/s Show Material materials with Difusividad térmica of 14.8 mm²/s | |
100.0 °C | 13.6 mm²/s Show Material materials with Difusividad térmica of 13.6 mm²/s | ||
200.0 °C | 12.1 mm²/s Show Material materials with Difusividad térmica of 12.1 mm²/s | ||
300.0 °C | 10.6 mm²/s Show Material materials with Difusividad térmica of 10.6 mm²/s | ||
400.0 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | ||
500.0 °C | 7.7 mm²/s Show Material materials with Difusividad térmica of 7.7 mm²/s | ||
600.0 °C | 6.2 mm²/s Show Material materials with Difusividad térmica of 6.2 mm²/s | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 300 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 300 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.95E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.95E-7 Ω·m |
100.0 °C | 2.42E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.42E-7 Ω·m | |
200.0 °C | 3.14E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.14E-7 Ω·m | |
300.0 °C | 4.02E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.02E-7 Ω·m | |
400.0 °C | 5.02E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.02E-7 Ω·m | |
500.0 °C | 6.21E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.21E-7 Ω·m | |
600.0 °C | 7.55E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.55E-7 Ω·m | |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % |
Azufre | 0.04 % Show Material materials with Azufre of 0.04 % |
Carbono | 0.2 % Show Material materials with Carbono of 0.2 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 0.4 % Show Material materials with Manganeso of 0.4 % |
Silicona | 0.35 % Show Material materials with Silicona of 0.35 % |