Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ |
50.0 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | |
100.0 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ | |
150.0 °C | 7.81 g/cm³ Show Material materials with Densidad of 7.81 g/cm³ | |
200.0 °C | 7.79 g/cm³ Show Material materials with Densidad of 7.79 g/cm³ | |
250.0 °C | 7.78 g/cm³ Show Material materials with Densidad of 7.78 g/cm³ | |
300.0 °C | 7.76 g/cm³ Show Material materials with Densidad of 7.76 g/cm³ | |
350.0 °C | 7.74 g/cm³ Show Material materials with Densidad of 7.74 g/cm³ | |
400.0 °C | 7.72 g/cm³ Show Material materials with Densidad of 7.72 g/cm³ | |
450.0 °C | 7.7 g/cm³ Show Material materials with Densidad of 7.7 g/cm³ | |
500.0 °C | 7.68 g/cm³ Show Material materials with Densidad of 7.68 g/cm³ | |
550.0 °C | 7.66 g/cm³ Show Material materials with Densidad of 7.66 g/cm³ | |
600.0 °C | 7.64 g/cm³ Show Material materials with Densidad of 7.64 g/cm³ | |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] |
50.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
100.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
150.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
250.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
300.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
350.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
450.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
500.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
550.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
600.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
Elongación | 20.0 °C | 21 % Show Material materials with Elongación of 21 % |
Elongación transversal | 20.0 °C | 19 % Show Material materials with Elongación transversal of 19 % |
Límite elástico Rp 0,2 | 20.0 °C | 235 - 255 MPa Show Material materials with Límite elástico Rp 0,2 of 235 - 255 MPa |
200.0 °C | 190 - 205 MPa Show Material materials with Límite elástico Rp 0,2 of 190 - 205 MPa | |
250.0 °C | 170 - 185 MPa Show Material materials with Límite elástico Rp 0,2 of 170 - 185 MPa | |
300.0 °C | 150 - 160 MPa Show Material materials with Límite elástico Rp 0,2 of 150 - 160 MPa | |
350.0 °C | 135 - 140 MPa Show Material materials with Límite elástico Rp 0,2 of 135 - 140 MPa | |
400.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | |
450.0 °C | 125 MPa Show Material materials with Límite elástico Rp 0,2 of 125 MPa | |
Módulo de cizallamiento | 20.0 °C | 82.31 GPa Show Material materials with Módulo de cizallamiento of 82.31 GPa |
50.0 °C | 81.62 GPa Show Material materials with Módulo de cizallamiento of 81.62 GPa | |
100.0 °C | 80.34 GPa Show Material materials with Módulo de cizallamiento of 80.34 GPa | |
150.0 °C | 78.97 GPa Show Material materials with Módulo de cizallamiento of 78.97 GPa | |
200.0 °C | 77.4 GPa Show Material materials with Módulo de cizallamiento of 77.4 GPa | |
250.0 °C | 75.83 GPa Show Material materials with Módulo de cizallamiento of 75.83 GPa | |
300.0 °C | 74.16 GPa Show Material materials with Módulo de cizallamiento of 74.16 GPa | |
350.0 °C | 72.5 GPa Show Material materials with Módulo de cizallamiento of 72.5 GPa | |
400.0 °C | 70.73 GPa Show Material materials with Módulo de cizallamiento of 70.73 GPa | |
450.0 °C | 69.06 GPa Show Material materials with Módulo de cizallamiento of 69.06 GPa | |
500.0 °C | 67.3 GPa Show Material materials with Módulo de cizallamiento of 67.3 GPa | |
550.0 °C | 65.53 GPa Show Material materials with Módulo de cizallamiento of 65.53 GPa | |
600.0 °C | 63.67 GPa Show Material materials with Módulo de cizallamiento of 63.67 GPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa |
20.0 °C | 211.31 - 212 GPa Show Material materials with Módulo elástico of 211.31 - 212 GPa | |
50.0 °C | 209.84 GPa Show Material materials with Módulo elástico of 209.84 GPa | |
100.0 °C | 206.79 - 207 GPa Show Material materials with Módulo elástico of 206.79 - 207 GPa | |
150.0 °C | 203.36 GPa Show Material materials with Módulo elástico of 203.36 GPa | |
200.0 °C | 199 - 200 GPa Show Material materials with Módulo elástico of 199 - 200 GPa | |
250.0 °C | 195.42 GPa Show Material materials with Módulo elástico of 195.42 GPa | |
300.0 °C | 191.49 - 192 GPa Show Material materials with Módulo elástico of 191.49 - 192 GPa | |
350.0 °C | 187.47 GPa Show Material materials with Módulo elástico of 187.47 GPa | |
400.0 °C | 183 - 184 GPa Show Material materials with Módulo elástico of 183 - 184 GPa | |
450.0 °C | 179.03 GPa Show Material materials with Módulo elástico of 179.03 GPa | |
500.0 °C | 174.72 - 175 GPa Show Material materials with Módulo elástico of 174.72 - 175 GPa | |
550.0 °C | 170.2 GPa Show Material materials with Módulo elástico of 170.2 GPa | |
600.0 °C | 164 - 166 GPa Show Material materials with Módulo elástico of 164 - 166 GPa | |
Resistencia a la tracción | 20.0 °C | 410 - 530 MPa Show Material materials with Resistencia a la tracción of 410 - 530 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 - 500 J/(kg·K) Show Material materials with Calor específico of 479 - 500 J/(kg·K) | ||
200.0 °C | 499 - 540 J/(kg·K) Show Material materials with Calor específico of 499 - 540 J/(kg·K) | ||
300.0 °C | 517 - 580 J/(kg·K) Show Material materials with Calor específico of 517 - 580 J/(kg·K) | ||
400.0 °C | 536 - 620 J/(kg·K) Show Material materials with Calor específico of 536 - 620 J/(kg·K) | ||
500.0 °C | 558 - 690 J/(kg·K) Show Material materials with Calor específico of 558 - 690 J/(kg·K) | ||
600.0 °C | 587 - 780 J/(kg·K) Show Material materials with Calor específico of 587 - 780 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
100.0 °C | 1.22E-5 - 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22E-5 - 1.25E-5 1/K | ||
200.0 °C | 1.29E-5 - 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29E-5 - 1.3E-5 1/K | ||
300.0 °C | 1.34E-5 - 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.34E-5 - 1.36E-5 1/K | ||
400.0 °C | 1.4E-5 - 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 - 1.41E-5 1/K | ||
500.0 °C | 1.43E-5 - 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.43E-5 - 1.45E-5 1/K | ||
600.0 °C | 1.46E-5 - 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.46E-5 - 1.49E-5 1/K | ||
Conductividad térmica | 20.0 °C | 53.4 W/(m·K) Show Material materials with Conductividad térmica of 53.4 W/(m·K) | |
100.0 °C | 52.9 - 53 W/(m·K) Show Material materials with Conductividad térmica of 52.9 - 53 W/(m·K) | ||
200.0 °C | 50 - 50.3 W/(m·K) Show Material materials with Conductividad térmica of 50 - 50.3 W/(m·K) | ||
300.0 °C | 46.7 - 47 W/(m·K) Show Material materials with Conductividad térmica of 46.7 - 47 W/(m·K) | ||
400.0 °C | 43 - 43.3 W/(m·K) Show Material materials with Conductividad térmica of 43 - 43.3 W/(m·K) | ||
500.0 °C | 39.8 - 40 W/(m·K) Show Material materials with Conductividad térmica of 39.8 - 40 W/(m·K) | ||
600.0 °C | 36 - 36.7 W/(m·K) Show Material materials with Conductividad térmica of 36 - 36.7 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 14.8 mm²/s Show Material materials with Difusividad térmica of 14.8 mm²/s | |
100.0 °C | 13.6 mm²/s Show Material materials with Difusividad térmica of 13.6 mm²/s | ||
200.0 °C | 12.1 mm²/s Show Material materials with Difusividad térmica of 12.1 mm²/s | ||
300.0 °C | 10.6 mm²/s Show Material materials with Difusividad térmica of 10.6 mm²/s | ||
400.0 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | ||
500.0 °C | 7.7 mm²/s Show Material materials with Difusividad térmica of 7.7 mm²/s | ||
600.0 °C | 6.2 mm²/s Show Material materials with Difusividad térmica of 6.2 mm²/s | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 500 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 500 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.95E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.95E-7 Ω·m |
50.0 °C | 2.11E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.11E-7 Ω·m | |
100.0 °C | 2.3E-7 - 2.42E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.3E-7 - 2.42E-7 Ω·m | |
150.0 °C | 2.76E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.76E-7 Ω·m | |
200.0 °C | 3E-7 - 3.14E-7 Ω·m Show Material materials with Resistividad eléctrica of 3E-7 - 3.14E-7 Ω·m | |
250.0 °C | 3.55E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.55E-7 Ω·m | |
300.0 °C | 3.8E-7 - 4.02E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.8E-7 - 4.02E-7 Ω·m | |
350.0 °C | 4.49E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.49E-7 Ω·m | |
400.0 °C | 4.8E-7 - 5.02E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.8E-7 - 5.02E-7 Ω·m | |
450.0 °C | 5.59E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.59E-7 Ω·m | |
500.0 °C | 6E-7 - 6.21E-7 Ω·m Show Material materials with Resistividad eléctrica of 6E-7 - 6.21E-7 Ω·m | |
550.0 °C | 6.83E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.83E-7 Ω·m | |
600.0 °C | 7.4E-7 - 7.55E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.4E-7 - 7.55E-7 Ω·m | |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Azufre | 0.04 % Show Material materials with Azufre of 0.04 % |
Carbono | 0.21 % Show Material materials with Carbono of 0.21 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 0.4 - 1.2 % Show Material materials with Manganeso of 0.4 - 1.2 % |
Silicona | 0.1 - 0.35 % Show Material materials with Silicona of 0.1 - 0.35 % |