General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Chromium Molybdenum Steel | ||||
Dureza Brinell | 231 [-] Show Material materials with Dureza Brinell of 231 [-] | Predicted Value, Transverse | ||||
Elongación | 15.1 % Show Material materials with Elongación of 15.1 % | Predicted Value, A200 | ||||
16.2 % Show Material materials with Elongación of 16.2 % | Predicted Value, A80 | |||||
16.8 % Show Material materials with Elongación of 16.8 % | Predicted Value, A80 Transverse | |||||
18.0 % Show Material materials with Elongación of 18.0 % | Predicted Value, A5 | |||||
19.4 % Show Material materials with Elongación of 19.4 % | Predicted Value, A50 | |||||
20 °C | 18 % Show Material materials with Elongación of 18 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | Transverse | |
Estricción | 20 °C | 50 % Show Material materials with Estricción of 50 % | quenched and tempered (+QT) | EN 10028-2 | Sheet | Transverse |
Límite elástico | 247.1 MPa Show Material materials with Límite elástico of 247.1 MPa | Predicted Value, RP1 Transverse | ||||
275.1 MPa Show Material materials with Límite elástico of 275.1 MPa | Predicted Value, RP1 | |||||
376.1 MPa Show Material materials with Límite elástico of 376.1 MPa | Predicted Value, Transverse | |||||
388 MPa Show Material materials with Límite elástico of 388 MPa | Predicted Value, RP05 | |||||
614.7 MPa Show Material materials with Límite elástico of 614.7 MPa | Predicted Value, RP002 | |||||
20 °C | 330 MPa Show Material materials with Límite elástico of 330 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | RP02 Transverse | |
50 °C | 341 MPa Show Material materials with Límite elástico of 341 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
100 °C | 320 MPa Show Material materials with Límite elástico of 320 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
100 °C | 323 MPa Show Material materials with Límite elástico of 323 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
100 °C | 338 MPa Show Material materials with Límite elástico of 338 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
150 °C | 311 MPa Show Material materials with Límite elástico of 311 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
200 °C | 300 MPa Show Material materials with Límite elástico of 300 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
200 °C | 303 MPa Show Material materials with Límite elástico of 303 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
200 °C | 319 MPa Show Material materials with Límite elástico of 319 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
250 °C | 280 MPa Show Material materials with Límite elástico of 280 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
250 °C | 298 MPa Show Material materials with Límite elástico of 298 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
250 °C | 309 MPa Show Material materials with Límite elástico of 309 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
300 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
300 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
300 °C | 304 MPa Show Material materials with Límite elástico of 304 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
350 °C | 270 MPa Show Material materials with Límite elástico of 270 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
350 °C | 292 MPa Show Material materials with Límite elástico of 292 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
350 °C | 294 MPa Show Material materials with Límite elástico of 294 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
400 °C | 260 MPa Show Material materials with Límite elástico of 260 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
400 °C | 284 MPa Show Material materials with Límite elástico of 284 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
400 °C | 287 MPa Show Material materials with Límite elástico of 287 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
400 °C | 287 MPa Show Material materials with Límite elástico of 287 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
450 °C | 250 MPa Show Material materials with Límite elástico of 250 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
450 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
450 °C | 279 MPa Show Material materials with Límite elástico of 279 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
450 °C | 279 MPa Show Material materials with Límite elástico of 279 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
Módulo de cizallamiento | 81.1 GPa Show Material materials with Módulo de cizallamiento of 81.1 GPa | Predicted Value | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
Resistencia a la tracción | 20 °C | 520 - 690 MPa Show Material materials with Resistencia a la tracción of 520 - 690 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | Transverse |
20 °C | 520 - 670 MPa Show Material materials with Resistencia a la tracción of 520 - 670 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | Transverse | |
20 °C | 540 - 690 MPa Show Material materials with Resistencia a la tracción of 540 - 690 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | Transverse | |
20 °C | 540 - 670 MPa Show Material materials with Resistencia a la tracción of 540 - 670 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | Transverse | |
Resistencia al cizallamiento | 669.4 MPa Show Material materials with Resistencia al cizallamiento of 669.4 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.05e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
20 °C | 1.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
Conductividad térmica | 20 °C | 34.9 W/(m·K) Show Material materials with Conductividad térmica of 34.9 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
100 °C | 37.3 W/(m·K) Show Material materials with Conductividad térmica of 37.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 38.2 W/(m·K) Show Material materials with Conductividad térmica of 38.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 37.8 W/(m·K) Show Material materials with Conductividad térmica of 37.8 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 36.6 W/(m·K) Show Material materials with Conductividad térmica of 36.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 35.2 W/(m·K) Show Material materials with Conductividad térmica of 35.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 33.6 W/(m·K) Show Material materials with Conductividad térmica of 33.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
Difusividad térmica | 20 °C | 9.7 mm²/s Show Material materials with Difusividad térmica of 9.7 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
100 °C | 9.6 mm²/s Show Material materials with Difusividad térmica of 9.6 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 8.5 mm²/s Show Material materials with Difusividad térmica of 8.5 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 7.8 mm²/s Show Material materials with Difusividad térmica of 7.8 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 6.8 mm²/s Show Material materials with Difusividad térmica of 6.8 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | ||||
Temperatura máx. de funcionamiento | 20 - 450 °C Show Material materials with Temperatura máx. de funcionamiento of 20 - 450 °C | quenched and tempered (+QT) | EN 10028-2 | Flat | Long |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 3 S/m Show Material materials with Conductividad eléctrica of 3 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 2.98e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.98e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
100 °C | 3.43e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.43e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 4.13e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.13e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 4.97e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.97e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 5.95e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.95e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 7.03e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.03e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 8.25e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.25e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.01 - 0.04 % Show Material materials with Aluminio of 0.01 - 0.04 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
0.01 - 0.035 % Show Material materials with Aluminio of 0.01 - 0.035 % | quenched and tempered (+QT) | EN 10028-2 | Sheet | |
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
0.012 % Show Material materials with Azufre of 0.012 % | quenched and tempered (+QT) | EN 10028-2 | Sheet | |
Carbono | 0.1 - 0.15 % Show Material materials with Carbono of 0.1 - 0.15 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Cobre | 0.2 % Show Material materials with Cobre of 0.2 % | quenched and tempered (+QT) | EN 10028-2 | Sheet |
0.25 % Show Material materials with Cobre of 0.25 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
Cromo | 2 - 2.5 % Show Material materials with Cromo of 2 - 2.5 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Fósforo | 0.015 % Show Material materials with Fósforo of 0.015 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Manganeso | 0.3 - 0.8 % Show Material materials with Manganeso of 0.3 - 0.8 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Molibdeno | 0.9 - 1.1 % Show Material materials with Molibdeno of 0.9 - 1.1 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Níquel | 0.3 % Show Material materials with Níquel of 0.3 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |