General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Elongación | 20.0 °C | 10 - 14 % Show Material materials with Elongación of 10 - 14 % |
Límite elástico Rp 0,2 | 20.0 °C | 550 - 700 MPa Show Material materials with Límite elástico Rp 0,2 of 550 - 700 MPa |
Módulo elástico | 20.0 °C | 211 GPa Show Material materials with Módulo elástico of 211 GPa |
100.0 °C | 204 GPa Show Material materials with Módulo elástico of 204 GPa | |
200.0 °C | 196 GPa Show Material materials with Módulo elástico of 196 GPa | |
300.0 °C | 186 GPa Show Material materials with Módulo elástico of 186 GPa | |
Resistencia a la tracción | 20.0 °C | 750 - 1000 MPa Show Material materials with Resistencia a la tracción of 750 - 1000 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Coeficiente de dilatación térmica | 100.0 °C | 1.1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 1/K |
200.0 °C | 1.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2E-5 1/K | |
300.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | |
Temperatura máx. de funcionamiento, largo | 0 - 300 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 300 °C |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.27 - 0.34 % Show Material materials with Carbono of 0.27 - 0.34 % |
Cromo | 1.3 - 1.7 % Show Material materials with Cromo of 1.3 - 1.7 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Manganeso | 0.6 - 1 % Show Material materials with Manganeso of 0.6 - 1 % |
Molibdeno | 0.3 - 0.5 % Show Material materials with Molibdeno of 0.3 - 0.5 % |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % |
Vanadio | 0.05 - 0.15 % Show Material materials with Vanadio of 0.05 - 0.15 % |