General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Nickel Steel |
Elongación | 20.0 °C | 22 % Show Material materials with Elongación of 22 % | |
Límite elástico | 20.0 °C | 335 - 355 MPa Show Material materials with Límite elástico of 335 - 355 MPa | |
Módulo de cizallamiento | 23.0 °C | 76 GPa Show Material materials with Módulo de cizallamiento of 76 GPa | Typical for Nickel Steel |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | ||
200.0 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | ||
Resistencia a la tracción | 20.0 °C | 490 - 610 MPa Show Material materials with Resistencia a la tracción of 490 - 610 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44E-5 1/K | ||
Conductividad térmica | 20.0 °C | 42.5 W/(m·K) Show Material materials with Conductividad térmica of 42.5 W/(m·K) | |
100.0 °C | 43.5 W/(m·K) Show Material materials with Conductividad térmica of 43.5 W/(m·K) | ||
200.0 °C | 42.8 W/(m·K) Show Material materials with Conductividad térmica of 42.8 W/(m·K) | ||
300.0 °C | 40.9 W/(m·K) Show Material materials with Conductividad térmica of 40.9 W/(m·K) | ||
400.0 °C | 39 W/(m·K) Show Material materials with Conductividad térmica of 39 W/(m·K) | ||
500.0 °C | 36.4 W/(m·K) Show Material materials with Conductividad térmica of 36.4 W/(m·K) | ||
600.0 °C | 34.1 W/(m·K) Show Material materials with Conductividad térmica of 34.1 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 11.7 mm²/s Show Material materials with Difusividad térmica of 11.7 mm²/s | |
100.0 °C | 11.2 mm²/s Show Material materials with Difusividad térmica of 11.2 mm²/s | ||
200.0 °C | 10.3 mm²/s Show Material materials with Difusividad térmica of 10.3 mm²/s | ||
300.0 °C | 9.3 mm²/s Show Material materials with Difusividad térmica of 9.3 mm²/s | ||
400.0 °C | 8.3 mm²/s Show Material materials with Difusividad térmica of 8.3 mm²/s | ||
500.0 °C | 7 mm²/s Show Material materials with Difusividad térmica of 7 mm²/s | ||
600.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | ||
Temperatura de fusión | 1316 - 1595 °C Show Material materials with Temperatura de fusión of 1316 - 1595 °C | Typical for Nickel Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 2.45E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.45E-7 Ω·m |
100.0 °C | 2.94E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.94E-7 Ω·m | |
200.0 °C | 3.69E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.69E-7 Ω·m | |
300.0 °C | 4.59E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.59E-7 Ω·m | |
400.0 °C | 5.58E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.58E-7 Ω·m | |
500.0 °C | 6.79E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.79E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.13E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % |
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % |
Carbono | 0.16 % Show Material materials with Carbono of 0.16 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.85 - 1.65 % Show Material materials with Manganeso of 0.85 - 1.65 % |
Niobio | 0.05 % Show Material materials with Niobio of 0.05 % |
Níquel | 0.3 - 0.85 % Show Material materials with Níquel of 0.3 - 0.85 % |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % |
Vanadio | 0.05 % Show Material materials with Vanadio of 0.05 % |