General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8 g/cm³ Show Material materials with Densidad of 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación | 20.0 °C | 30 % Show Material materials with Elongación of 30 % | |
Límite elástico Rp 1,0 | 20.0 °C | 190 MPa Show Material materials with Límite elástico Rp 1,0 of 190 MPa | |
100.0 °C | 165 MPa Show Material materials with Límite elástico Rp 1,0 of 165 MPa | ||
200.0 °C | 135 MPa Show Material materials with Límite elástico Rp 1,0 of 135 MPa | ||
300.0 °C | 120 MPa Show Material materials with Límite elástico Rp 1,0 of 120 MPa | ||
400.0 °C | 110 MPa Show Material materials with Límite elástico Rp 1,0 of 110 MPa | ||
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | 23.0 °C | 195 GPa Show Material materials with Módulo elástico of 195 GPa | Typical for Austenitic Stainless Steel |
Resistencia a la tracción | 20.0 °C | 430 - 630 MPa Show Material materials with Resistencia a la tracción of 430 - 630 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 1/K | |
300.0 °C | 1.62E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.62E-5 1/K | ||
500.0 °C | 1.7E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K | ||
Conductividad térmica | 50.0 °C | 16 W/(m·K) Show Material materials with Conductividad térmica of 16 W/(m·K) | |
100.0 °C | 17 W/(m·K) Show Material materials with Conductividad térmica of 17 W/(m·K) | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Resistividad eléctrica | 23.0 °C | 8.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % |
Carbono | 0.03 % Show Material materials with Carbono of 0.03 % |
Cobre | 2 % Show Material materials with Cobre of 2 % |
Cromo | 19 - 22 % Show Material materials with Cromo of 19 - 22 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 2 - 2.5 % Show Material materials with Molibdeno of 2 - 2.5 % |
Nitrógeno | 0.2 % Show Material materials with Nitrógeno of 0.2 % |
Níquel | 26 - 30 % Show Material materials with Níquel of 26 - 30 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |