General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.1 g/cm³ Show Material materials with Densidad of 7.1 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.26 [-] Show Material materials with Coeficiente de Poisson of 0.26 [-] | |
Dureza Brinell | 20.0 °C | 205 - 270 [-] Show Material materials with Dureza Brinell of 205 - 270 [-] | |
Módulo de cizallamiento | 23.0 °C | 41 GPa Show Material materials with Módulo de cizallamiento of 41 GPa | Typical for Cast Iron |
Módulo elástico | 20.0 °C | 78 - 103 GPa Show Material materials with Módulo elástico of 78 - 103 GPa | |
Plane-Strain Fracture Toughnes | 20.0 °C | 10.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 10.1 MPa·√m | |
Resistencia a la tracción | 20.0 °C | 80 - 200 MPa Show Material materials with Resistencia a la tracción of 80 - 200 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 200.0 °C | 460 J/(kg·K) Show Material materials with Calor específico of 460 J/(kg·K) | |
600.0 °C | 535 J/(kg·K) Show Material materials with Calor específico of 535 J/(kg·K) | ||
Conductividad térmica | 100.0 °C | 52.5 W/(m·K) Show Material materials with Conductividad térmica of 52.5 W/(m·K) | |
200.0 °C | 51 W/(m·K) Show Material materials with Conductividad térmica of 51 W/(m·K) | ||
300.0 °C | 50 W/(m·K) Show Material materials with Conductividad térmica of 50 W/(m·K) | ||
400.0 °C | 49 W/(m·K) Show Material materials with Conductividad térmica of 49 W/(m·K) | ||
500.0 °C | 48.5 W/(m·K) Show Material materials with Conductividad térmica of 48.5 W/(m·K) | ||
Temperatura de fusión | 1120 °C Show Material materials with Temperatura de fusión of 1120 °C | Typical for Cast Iron |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 8E-7 Ω·m Show Material materials with Resistividad eléctrica of 8E-7 Ω·m |