General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.7 g/cm³ Show Material materials with Densidad of 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.27 [-] Show Material materials with Coeficiente de Poisson of 0.27 [-] | Typical for Cast Iron |
Dureza Brinell | 20.0 °C | 430 - 690 [-] Show Material materials with Dureza Brinell of 430 - 690 [-] | |
Dureza Vickers | 20.0 °C | 450 - 750 [-] Show Material materials with Dureza Vickers of 450 - 750 [-] | |
Módulo de cizallamiento | 23.0 °C | 41 GPa Show Material materials with Módulo de cizallamiento of 41 GPa | Typical for Cast Iron |
Módulo elástico | 20.0 °C | 196 GPa Show Material materials with Módulo elástico of 196 GPa | |
Resistencia a la tracción | 20.0 °C | 500 - 600 MPa Show Material materials with Resistencia a la tracción of 500 - 600 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | |
Coeficiente de dilatación térmica | 23.0 °C | 1.5E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.5E-5 1/K | Typical for White Cast Iron |
Conductividad térmica | 20.0 °C | 13.8 W/(m·K) Show Material materials with Conductividad térmica of 13.8 W/(m·K) | |
Temperatura de fusión | 1209 °C Show Material materials with Temperatura de fusión of 1209 °C | Typical for White Cast Iron |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 8.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Carbono | 2.5 - 3.5 % Show Material materials with Carbono of 2.5 - 3.5 % |
Cromo | 8 - 10 % Show Material materials with Cromo of 8 - 10 % |
Manganeso | 0.3 - 0.7 % Show Material materials with Manganeso of 0.3 - 0.7 % |
Molibdeno | 0.5 % Show Material materials with Molibdeno of 0.5 % |
Níquel | 4.5 - 6.5 % Show Material materials with Níquel of 4.5 - 6.5 % |