General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 7.15 g/cm³ Show Material materials with Densidad of 7.15 g/cm³ | Typical for Ductile (Nodular) Cast Iron |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.27 - 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.27 - 0.29 [-] | |
Compressive yield strength | 20.0 °C | 870 MPa Show Material materials with Compressive yield strength of 870 MPa | |
Dureza Brinell | 20.0 °C | 200 - 250 [-] Show Material materials with Dureza Brinell of 200 - 250 [-] | |
Elongación | 20.0 °C | 3 % Show Material materials with Elongación of 3 % | |
Límite elástico | 20.0 °C | 380 MPa Show Material materials with Límite elástico of 380 MPa | |
Módulo de cizallamiento | 23.0 °C | 63 - 66 GPa Show Material materials with Módulo de cizallamiento of 63 - 66 GPa | Typical for Ductile (Nodular) Cast Iron |
Módulo elástico | 23.0 °C | 165 - 180 GPa Show Material materials with Módulo elástico of 165 - 180 GPa | Typical for Ductile (Nodular) Cast Iron |
Resistencia a la tracción | 20.0 °C | 600 MPa Show Material materials with Resistencia a la tracción of 600 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 460 - 502 J/(kg·K) Show Material materials with Calor específico of 460 - 502 J/(kg·K) | Typical for Ductile (Nodular) Cast Iron |
Coeficiente de dilatación térmica | 100.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | |
200.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | ||
300.0 °C | 1.35E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.35E-5 1/K | ||
400.0 °C | 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 1/K | ||
Conductividad térmica | 100.0 °C | 33 W/(m·K) Show Material materials with Conductividad térmica of 33 W/(m·K) | |
200.0 °C | 34 W/(m·K) Show Material materials with Conductividad térmica of 34 W/(m·K) | ||
300.0 °C | 33 W/(m·K) Show Material materials with Conductividad térmica of 33 W/(m·K) | ||
400.0 °C | 32 W/(m·K) Show Material materials with Conductividad térmica of 32 W/(m·K) | ||
500.0 °C | 30 W/(m·K) Show Material materials with Conductividad térmica of 30 W/(m·K) | ||
Temperatura de fusión | 1150 - 1200 °C Show Material materials with Temperatura de fusión of 1150 - 1200 °C | Typical for Ductile (Nodular) Cast Iron |
Chemical properties
Property | Value |
---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % |
Carbono | 3.5 - 3.8 % Show Material materials with Carbono of 3.5 - 3.8 % |
Fósforo | 0.1 % Show Material materials with Fósforo of 0.1 % |
Magnesio | 0.06 - 0.12 % Show Material materials with Magnesio of 0.06 - 0.12 % |
Manganeso | 0.4 % Show Material materials with Manganeso of 0.4 % |
Silicona | 2 - 3 % Show Material materials with Silicona of 2 - 3 % |