General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.9 g/cm³ Show Material materials with Densidad of 7.9 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Elongación | 20.0 °C | 20 % Show Material materials with Elongación of 20 % |
Límite elástico Rp 0,2 | 20.0 °C | 315 MPa Show Material materials with Límite elástico Rp 0,2 of 315 MPa |
100.0 °C | 220 MPa Show Material materials with Límite elástico Rp 0,2 of 220 MPa | |
200.0 °C | 170 MPa Show Material materials with Límite elástico Rp 0,2 of 170 MPa | |
300.0 °C | 140 MPa Show Material materials with Límite elástico Rp 0,2 of 140 MPa | |
350.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | |
400.0 °C | 120 MPa Show Material materials with Límite elástico Rp 0,2 of 120 MPa | |
Límite elástico Rp 1,0 | 20.0 °C | 340 MPa Show Material materials with Límite elástico Rp 1,0 of 340 MPa |
Resistencia a la tracción | 20.0 °C | 570 - 800 MPa Show Material materials with Resistencia a la tracción of 570 - 800 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 20.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) |
Coeficiente de dilatación térmica | 100.0 °C | 1.57E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.57E-5 1/K |
200.0 °C | 1.7E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K | |
300.0 °C | 1.75E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 1/K | |
Conductividad térmica | 20.0 °C | 14 W/(m·K) Show Material materials with Conductividad térmica of 14 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % |
Carbono | 0.03 % Show Material materials with Carbono of 0.03 % |
Cromo | 20 - 22 % Show Material materials with Cromo of 20 - 22 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 3 - 6 % Show Material materials with Manganeso of 3 - 6 % |
Molibdeno | 3 - 3.5 % Show Material materials with Molibdeno of 3 - 3.5 % |
Niobio | 0.25 % Show Material materials with Niobio of 0.25 % |
Nitrógeno | 0.2 - 0.35 % Show Material materials with Nitrógeno of 0.2 - 0.35 % |
Níquel | 14 - 17 % Show Material materials with Níquel of 14 - 17 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |