General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | |
Dureza Brinell | 270 [-] Show Material materials with Dureza Brinell of 270 [-] | Predicted Value, Transverse | ||||
Elongación | 14.3 % Show Material materials with Elongación of 14.3 % | Predicted Value, A200 | ||||
19.1 % Show Material materials with Elongación of 19.1 % | Predicted Value, A50 | |||||
20.9 % Show Material materials with Elongación of 20.9 % | Predicted Value, A5 | |||||
20 °C | 10 % Show Material materials with Elongación of 10 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | A80 Transverse | |
20 °C | 11 % Show Material materials with Elongación of 11 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | A80 Transverse | |
20 °C | 12 % Show Material materials with Elongación of 12 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | A80 Transverse | |
20 °C | 12 % Show Material materials with Elongación of 12 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 13 % Show Material materials with Elongación of 13 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | A80 Transverse | |
20 °C | 13 % Show Material materials with Elongación of 13 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 14 % Show Material materials with Elongación of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | A80 Transverse | |
20 °C | 14 % Show Material materials with Elongación of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | Transverse | |
20 °C | 14 % Show Material materials with Elongación of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | Transverse | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | Transverse | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | Transverse | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | Transverse | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
Estricción | 41.4 % Show Material materials with Estricción of 41.4 % | Predicted Value | ||||
42.5 % Show Material materials with Estricción of 42.5 % | Predicted Value, Transverse | |||||
Límite elástico | 307 MPa Show Material materials with Límite elástico of 307 MPa | Predicted Value, RP1 Transverse | ||||
311.3 MPa Show Material materials with Límite elástico of 311.3 MPa | Predicted Value, RP1 | |||||
326.4 MPa Show Material materials with Límite elástico of 326.4 MPa | Predicted Value, RP05 | |||||
401.4 MPa Show Material materials with Límite elástico of 401.4 MPa | Predicted Value, Transverse | |||||
498.6 MPa Show Material materials with Límite elástico of 498.6 MPa | Predicted Value, RP02 Transverse | |||||
523.8 MPa Show Material materials with Límite elástico of 523.8 MPa | Predicted Value, RP02 | |||||
619.6 MPa Show Material materials with Límite elástico of 619.6 MPa | Predicted Value, RP002 | |||||
20 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 245 MPa Show Material materials with Límite elástico of 245 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 255 MPa Show Material materials with Límite elástico of 255 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 265 MPa Show Material materials with Límite elástico of 265 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
Resistencia a la tracción | 20 °C | 440 - 660 MPa Show Material materials with Resistencia a la tracción of 440 - 660 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 440 - 610 MPa Show Material materials with Resistencia a la tracción of 440 - 610 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 450 - 660 MPa Show Material materials with Resistencia a la tracción of 450 - 660 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 450 - 610 MPa Show Material materials with Resistencia a la tracción of 450 - 610 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 660 MPa Show Material materials with Resistencia a la tracción of 470 - 660 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 610 MPa Show Material materials with Resistencia a la tracción of 470 - 610 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 490 - 660 MPa Show Material materials with Resistencia a la tracción of 490 - 660 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 490 - 610 MPa Show Material materials with Resistencia a la tracción of 490 - 610 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
Resistencia al cizallamiento | 552.2 MPa Show Material materials with Resistencia al cizallamiento of 552.2 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
Conductividad térmica | 20 °C | 53.4 W/(m·K) Show Material materials with Conductividad térmica of 53.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | |
100 °C | 52.9 W/(m·K) Show Material materials with Conductividad térmica of 52.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
200 °C | 50.3 W/(m·K) Show Material materials with Conductividad térmica of 50.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
300 °C | 46.7 W/(m·K) Show Material materials with Conductividad térmica of 46.7 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
400 °C | 43.3 W/(m·K) Show Material materials with Conductividad térmica of 43.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
500 °C | 39.8 W/(m·K) Show Material materials with Conductividad térmica of 39.8 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
600 °C | 36.7 W/(m·K) Show Material materials with Conductividad térmica of 36.7 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
Difusividad térmica | 20 °C | 14.8 mm²/s Show Material materials with Difusividad térmica of 14.8 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | |
100 °C | 13.6 mm²/s Show Material materials with Difusividad térmica of 13.6 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
200 °C | 12.1 mm²/s Show Material materials with Difusividad térmica of 12.1 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
300 °C | 10.6 mm²/s Show Material materials with Difusividad térmica of 10.6 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
400 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
500 °C | 7.7 mm²/s Show Material materials with Difusividad térmica of 7.7 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
600 °C | 6.2 mm²/s Show Material materials with Difusividad térmica of 6.2 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 330.4 °C Show Material materials with Temperatura máx. de funcionamiento of 330.4 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 8 S/m Show Material materials with Conductividad eléctrica of 8 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 1.95e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.95e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | |
100 °C | 2.42e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.42e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
200 °C | 3.14e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.14e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
300 °C | 4.02e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.02e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
400 °C | 5.02e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.02e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
500 °C | 6.21e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.21e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire | ||
600 °C | 7.55e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.55e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.045 % Show Material materials with Azufre of 0.045 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire |
Fósforo | 0.045 % Show Material materials with Fósforo of 0.045 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025, EN 10025-1 | Sheet, Strip, Flat, Rod, Wire |