General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
20 °C | 7.8 - 7.85 g/cm³ Show Material materials with Densidad of 7.8 - 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
Dureza Brinell | 245 [-] Show Material materials with Dureza Brinell of 245 [-] | Predicted Value, Transverse | ||||
Elongación | 15.2 % Show Material materials with Elongación of 15.2 % | Predicted Value, A200 | ||||
16.5 % Show Material materials with Elongación of 16.5 % | Predicted Value, A80 | |||||
18.9 % Show Material materials with Elongación of 18.9 % | Predicted Value, A5 | |||||
19.4 % Show Material materials with Elongación of 19.4 % | Predicted Value, A50 | |||||
20.2 % Show Material materials with Elongación of 20.2 % | Predicted Value, A80 Transverse | |||||
20 °C | 24 % Show Material materials with Elongación of 24 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 24 % Show Material materials with Elongación of 24 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Estricción | 41.4 % Show Material materials with Estricción of 41.4 % | Predicted Value | ||||
42.4 % Show Material materials with Estricción of 42.4 % | Predicted Value, Transverse | |||||
Límite elástico | 285.7 MPa Show Material materials with Límite elástico of 285.7 MPa | Predicted Value, RP1 Transverse | ||||
295.4 MPa Show Material materials with Límite elástico of 295.4 MPa | Predicted Value, RP1 | |||||
359.7 MPa Show Material materials with Límite elástico of 359.7 MPa | Predicted Value, RP05 | |||||
413.1 MPa Show Material materials with Límite elástico of 413.1 MPa | Predicted Value, RP02 Transverse | |||||
592.9 MPa Show Material materials with Límite elástico of 592.9 MPa | Predicted Value, RP002 | |||||
20 °C | 170 MPa Show Material materials with Límite elástico of 170 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 170 MPa Show Material materials with Límite elástico of 170 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 185 MPa Show Material materials with Límite elástico of 185 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 185 MPa Show Material materials with Límite elástico of 185 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 200 MPa Show Material materials with Límite elástico of 200 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 200 MPa Show Material materials with Límite elástico of 200 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
50 °C | 164 MPa Show Material materials with Límite elástico of 164 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 179 MPa Show Material materials with Límite elástico of 179 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 193 MPa Show Material materials with Límite elástico of 193 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 208 MPa Show Material materials with Límite elástico of 208 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 218 MPa Show Material materials with Límite elástico of 218 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 227 MPa Show Material materials with Límite elástico of 227 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 155 MPa Show Material materials with Límite elástico of 155 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 168 MPa Show Material materials with Límite elástico of 168 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 182 MPa Show Material materials with Límite elástico of 182 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 196 MPa Show Material materials with Límite elástico of 196 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 205 MPa Show Material materials with Límite elástico of 205 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 214 MPa Show Material materials with Límite elástico of 214 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 143 MPa Show Material materials with Límite elástico of 143 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 156 MPa Show Material materials with Límite elástico of 156 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 169 MPa Show Material materials with Límite elástico of 169 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 181 MPa Show Material materials with Límite elástico of 181 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 190 MPa Show Material materials with Límite elástico of 190 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 198 MPa Show Material materials with Límite elástico of 198 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 132 MPa Show Material materials with Límite elástico of 132 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 143 MPa Show Material materials with Límite elástico of 143 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 155 MPa Show Material materials with Límite elástico of 155 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 167 MPa Show Material materials with Límite elástico of 167 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 174 MPa Show Material materials with Límite elástico of 174 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 182 MPa Show Material materials with Límite elástico of 182 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 121 MPa Show Material materials with Límite elástico of 121 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 131 MPa Show Material materials with Límite elástico of 131 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 142 MPa Show Material materials with Límite elástico of 142 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 153 MPa Show Material materials with Límite elástico of 153 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 160 MPa Show Material materials with Límite elástico of 160 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 167 MPa Show Material materials with Límite elástico of 167 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 111 MPa Show Material materials with Límite elástico of 111 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 121 MPa Show Material materials with Límite elástico of 121 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 130 MPa Show Material materials with Límite elástico of 130 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 140 MPa Show Material materials with Límite elástico of 140 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 147 MPa Show Material materials with Límite elástico of 147 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 153 MPa Show Material materials with Límite elástico of 153 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 103 MPa Show Material materials with Límite elástico of 103 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 112 MPa Show Material materials with Límite elástico of 112 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 121 MPa Show Material materials with Límite elástico of 121 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 130 MPa Show Material materials with Límite elástico of 130 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 136 MPa Show Material materials with Límite elástico of 136 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 142 MPa Show Material materials with Límite elástico of 142 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 97 MPa Show Material materials with Límite elástico of 97 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 105 MPa Show Material materials with Límite elástico of 105 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 114 MPa Show Material materials with Límite elástico of 114 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 122 MPa Show Material materials with Límite elástico of 122 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 128 MPa Show Material materials with Límite elástico of 128 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 133 MPa Show Material materials with Límite elástico of 133 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 210 GPa Show Material materials with Módulo elástico of 210 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 210 - 212 GPa Show Material materials with Módulo elástico of 210 - 212 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 205 GPa Show Material materials with Módulo elástico of 205 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 205 - 207 GPa Show Material materials with Módulo elástico of 205 - 207 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 195 GPa Show Material materials with Módulo elástico of 195 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 195 - 199 GPa Show Material materials with Módulo elástico of 195 - 199 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 185 GPa Show Material materials with Módulo elástico of 185 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 185 - 192 GPa Show Material materials with Módulo elástico of 185 - 192 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 175 - 184 GPa Show Material materials with Módulo elástico of 175 - 184 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Resistencia a la tracción | 20 °C | 340 - 480 MPa Show Material materials with Resistencia a la tracción of 340 - 480 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse |
20 °C | 340 - 480 MPa Show Material materials with Resistencia a la tracción of 340 - 480 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 350 - 480 MPa Show Material materials with Resistencia a la tracción of 350 - 480 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 350 - 480 MPa Show Material materials with Resistencia a la tracción of 350 - 480 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 360 - 480 MPa Show Material materials with Resistencia a la tracción of 360 - 480 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 360 - 480 MPa Show Material materials with Resistencia a la tracción of 360 - 480 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Resistencia al cizallamiento | 536 MPa Show Material materials with Resistencia al cizallamiento of 536 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 450 J/(kg·K) Show Material materials with Calor específico of 450 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 450 - 461 J/(kg·K) Show Material materials with Calor específico of 450 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Conductividad térmica | 20 °C | 46.8 W/(m·K) Show Material materials with Conductividad térmica of 46.8 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 46.8 - 57.5 W/(m·K) Show Material materials with Conductividad térmica of 46.8 - 57.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 57.5 W/(m·K) Show Material materials with Conductividad térmica of 57.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 43 W/(m·K) Show Material materials with Conductividad térmica of 43 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 43 - 55.7 W/(m·K) Show Material materials with Conductividad térmica of 43 - 55.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 55.7 W/(m·K) Show Material materials with Conductividad térmica of 55.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 40 W/(m·K) Show Material materials with Conductividad térmica of 40 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 40 - 51.9 W/(m·K) Show Material materials with Conductividad térmica of 40 - 51.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 51.9 W/(m·K) Show Material materials with Conductividad térmica of 51.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 36 W/(m·K) Show Material materials with Conductividad térmica of 36 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 36 - 47.6 W/(m·K) Show Material materials with Conductividad térmica of 36 - 47.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 47.6 W/(m·K) Show Material materials with Conductividad térmica of 47.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 32 W/(m·K) Show Material materials with Conductividad térmica of 32 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 32 - 43.4 W/(m·K) Show Material materials with Conductividad térmica of 32 - 43.4 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 43.4 W/(m·K) Show Material materials with Conductividad térmica of 43.4 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 29 W/(m·K) Show Material materials with Conductividad térmica of 29 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 29 - 39.6 W/(m·K) Show Material materials with Conductividad térmica of 29 - 39.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 39.6 W/(m·K) Show Material materials with Conductividad térmica of 39.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 36 W/(m·K) Show Material materials with Conductividad térmica of 36 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Difusividad térmica | 20 °C | 15.9 mm²/s Show Material materials with Difusividad térmica of 15.9 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
100 °C | 14.3 mm²/s Show Material materials with Difusividad térmica of 14.3 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 12.5 mm²/s Show Material materials with Difusividad térmica of 12.5 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 10.8 mm²/s Show Material materials with Difusividad térmica of 10.8 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 7.6 mm²/s Show Material materials with Difusividad térmica of 7.6 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 6.1 mm²/s Show Material materials with Difusividad térmica of 6.1 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 20 - 400 °C Show Material materials with Temperatura máx. de funcionamiento of 20 - 400 °C | normalized or normalized formed (+N) | EN 10028-2 | Flat | Long | |
400 °C Show Material materials with Temperatura máx. de funcionamiento of 400 °C | normalized or normalized formed (+N) | EN 10028-2 | Flat | Long | ||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 6 S/m Show Material materials with Conductividad eléctrica of 6 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 1.1e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.1e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
100 °C | 2.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.3e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.04e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.04e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 3.94e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.94e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.01e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.01e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.25e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.25e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.7e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
0.015 % Show Material materials with Azufre of 0.015 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
Carbono | 0.16 % Show Material materials with Carbono of 0.16 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Manganeso | 0.6 - 1.2 % Show Material materials with Manganeso of 0.6 - 1.2 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Molibdeno | 0.08 % Show Material materials with Molibdeno of 0.08 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Niobio | 0.02 % Show Material materials with Niobio of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Níquel | 0.3 % Show Material materials with Níquel of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Silicona | 0.35 % Show Material materials with Silicona of 0.35 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Vanadio | 0.02 % Show Material materials with Vanadio of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |