General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
20 °C | 7.83 - 7.84 g/cm³ Show Material materials with Densidad of 7.83 - 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel | ||||
Dureza Brinell | 244 [-] Show Material materials with Dureza Brinell of 244 [-] | Predicted Value, Transverse | ||||
Elongación | 15.4 % Show Material materials with Elongación of 15.4 % | Predicted Value, A200 | ||||
15.7 % Show Material materials with Elongación of 15.7 % | Predicted Value, A80 | |||||
16.6 % Show Material materials with Elongación of 16.6 % | Predicted Value, A80 Transverse | |||||
16.8 % Show Material materials with Elongación of 16.8 % | Predicted Value, A5 | |||||
19.2 % Show Material materials with Elongación of 19.2 % | Predicted Value, A50 | |||||
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Estricción | 42.0 % Show Material materials with Estricción of 42.0 % | Predicted Value | ||||
43.5 % Show Material materials with Estricción of 43.5 % | Predicted Value, Transverse | |||||
Límite elástico | 289.1 MPa Show Material materials with Límite elástico of 289.1 MPa | Predicted Value, RP1 Transverse | ||||
299.4 MPa Show Material materials with Límite elástico of 299.4 MPa | Predicted Value, RP1 | |||||
378.1 MPa Show Material materials with Límite elástico of 378.1 MPa | Predicted Value, RP05 | |||||
407.3 MPa Show Material materials with Límite elástico of 407.3 MPa | Predicted Value, RP02 Transverse | |||||
601.7 MPa Show Material materials with Límite elástico of 601.7 MPa | Predicted Value, RP002 | |||||
20 °C | 220 MPa Show Material materials with Límite elástico of 220 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 220 MPa Show Material materials with Límite elástico of 220 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 260 MPa Show Material materials with Límite elástico of 260 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 260 MPa Show Material materials with Límite elástico of 260 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 290 MPa Show Material materials with Límite elástico of 290 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 290 MPa Show Material materials with Límite elástico of 290 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
50 °C | 213 MPa Show Material materials with Límite elástico of 213 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 227 MPa Show Material materials with Límite elástico of 227 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 251 MPa Show Material materials with Límite elástico of 251 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 276 MPa Show Material materials with Límite elástico of 276 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 280 MPa Show Material materials with Límite elástico of 280 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 200 MPa Show Material materials with Límite elástico of 200 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 214 MPa Show Material materials with Límite elástico of 214 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 237 MPa Show Material materials with Límite elástico of 237 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 259 MPa Show Material materials with Límite elástico of 259 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 264 MPa Show Material materials with Límite elástico of 264 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 268 MPa Show Material materials with Límite elástico of 268 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 185 MPa Show Material materials with Límite elástico of 185 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 198 MPa Show Material materials with Límite elástico of 198 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 219 MPa Show Material materials with Límite elástico of 219 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 240 MPa Show Material materials with Límite elástico of 240 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 244 MPa Show Material materials with Límite elástico of 244 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 249 MPa Show Material materials with Límite elástico of 249 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 170 MPa Show Material materials with Límite elástico of 170 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 182 MPa Show Material materials with Límite elástico of 182 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 201 MPa Show Material materials with Límite elástico of 201 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 221 MPa Show Material materials with Límite elástico of 221 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 228 MPa Show Material materials with Límite elástico of 228 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 156 MPa Show Material materials with Límite elástico of 156 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 167 MPa Show Material materials with Límite elástico of 167 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 184 MPa Show Material materials with Límite elástico of 184 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 202 MPa Show Material materials with Límite elástico of 202 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 206 MPa Show Material materials with Límite elástico of 206 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 209 MPa Show Material materials with Límite elástico of 209 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 144 MPa Show Material materials with Límite elástico of 144 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 153 MPa Show Material materials with Límite elástico of 153 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 170 MPa Show Material materials with Límite elástico of 170 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 186 MPa Show Material materials with Límite elástico of 186 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 189 MPa Show Material materials with Límite elástico of 189 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 192 MPa Show Material materials with Límite elástico of 192 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 133 MPa Show Material materials with Límite elástico of 133 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 142 MPa Show Material materials with Límite elástico of 142 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 157 MPa Show Material materials with Límite elástico of 157 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 172 MPa Show Material materials with Límite elástico of 172 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 175 MPa Show Material materials with Límite elástico of 175 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 178 MPa Show Material materials with Límite elástico of 178 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 125 MPa Show Material materials with Límite elástico of 125 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 133 MPa Show Material materials with Límite elástico of 133 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 148 MPa Show Material materials with Límite elástico of 148 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 162 MPa Show Material materials with Límite elástico of 162 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 165 MPa Show Material materials with Límite elástico of 165 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 167 MPa Show Material materials with Límite elástico of 167 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 207 - 208 GPa Show Material materials with Módulo elástico of 207 - 208 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 208 GPa Show Material materials with Módulo elástico of 208 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 199 - 201 GPa Show Material materials with Módulo elástico of 199 - 201 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 201 GPa Show Material materials with Módulo elástico of 201 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 192 - 193 GPa Show Material materials with Módulo elástico of 192 - 193 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 193 GPa Show Material materials with Módulo elástico of 193 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 184 - 185 GPa Show Material materials with Módulo elástico of 184 - 185 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 185 GPa Show Material materials with Módulo elástico of 185 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Resistencia a la tracción | 20 °C | 430 - 580 MPa Show Material materials with Resistencia a la tracción of 430 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse |
20 °C | 430 - 570 MPa Show Material materials with Resistencia a la tracción of 430 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 430 - 580 MPa Show Material materials with Resistencia a la tracción of 430 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 430 - 570 MPa Show Material materials with Resistencia a la tracción of 430 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 440 - 580 MPa Show Material materials with Resistencia a la tracción of 440 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 440 - 570 MPa Show Material materials with Resistencia a la tracción of 440 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 440 - 580 MPa Show Material materials with Resistencia a la tracción of 440 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 440 - 570 MPa Show Material materials with Resistencia a la tracción of 440 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 460 - 580 MPa Show Material materials with Resistencia a la tracción of 460 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 460 - 570 MPa Show Material materials with Resistencia a la tracción of 460 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 460 - 580 MPa Show Material materials with Resistencia a la tracción of 460 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 460 - 570 MPa Show Material materials with Resistencia a la tracción of 460 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Resistencia al cizallamiento | 547.7 MPa Show Material materials with Resistencia al cizallamiento of 547.7 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Calor específico of 430 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Calor específico of 430 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Calor específico of 479 - 500 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Calor específico of 499 - 540 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 540 J/(kg·K) Show Material materials with Calor específico of 540 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 517 - 580 J/(kg·K) Show Material materials with Calor específico of 517 - 580 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 580 J/(kg·K) Show Material materials with Calor específico of 580 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Calor específico of 536 - 620 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 620 J/(kg·K) Show Material materials with Calor específico of 620 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 558 - 690 J/(kg·K) Show Material materials with Calor específico of 558 - 690 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 690 J/(kg·K) Show Material materials with Calor específico of 690 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 587 - 780 J/(kg·K) Show Material materials with Calor específico of 587 - 780 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 780 J/(kg·K) Show Material materials with Calor específico of 780 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 1.22e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 1.22e-05 - 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22e-05 - 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.29e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.29e-05 - 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29e-05 - 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.34e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.34e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.34e-05 - 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.34e-05 - 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.4e-05 - 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 - 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.43e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 - 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.43e-05 - 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.46e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.46e-05 - 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.46e-05 - 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Conductividad térmica | 20 °C | 46.5 - 47 W/(m·K) Show Material materials with Conductividad térmica of 46.5 - 47 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 46.5 W/(m·K) Show Material materials with Conductividad térmica of 46.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 47 W/(m·K) Show Material materials with Conductividad térmica of 47 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 47 W/(m·K) Show Material materials with Conductividad térmica of 47 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 47 - 47.2 W/(m·K) Show Material materials with Conductividad térmica of 47 - 47.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 47.2 W/(m·K) Show Material materials with Conductividad térmica of 47.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 45.9 - 46 W/(m·K) Show Material materials with Conductividad térmica of 45.9 - 46 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 45.9 W/(m·K) Show Material materials with Conductividad térmica of 45.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 46 W/(m·K) Show Material materials with Conductividad térmica of 46 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 43.5 - 44 W/(m·K) Show Material materials with Conductividad térmica of 43.5 - 44 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 43.5 W/(m·K) Show Material materials with Conductividad térmica of 43.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 44 W/(m·K) Show Material materials with Conductividad térmica of 44 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 40.9 - 41 W/(m·K) Show Material materials with Conductividad térmica of 40.9 - 41 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 40.9 W/(m·K) Show Material materials with Conductividad térmica of 40.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 41 W/(m·K) Show Material materials with Conductividad térmica of 41 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 38 W/(m·K) Show Material materials with Conductividad térmica of 38 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 38 - 38.1 W/(m·K) Show Material materials with Conductividad térmica of 38 - 38.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 38.1 W/(m·K) Show Material materials with Conductividad térmica of 38.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 35 W/(m·K) Show Material materials with Conductividad térmica of 35 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 35 - 35.3 W/(m·K) Show Material materials with Conductividad térmica of 35 - 35.3 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 35.3 W/(m·K) Show Material materials with Conductividad térmica of 35.3 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Difusividad térmica | 20 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
100 °C | 12.2 mm²/s Show Material materials with Difusividad térmica of 12.2 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 11.1 mm²/s Show Material materials with Difusividad térmica of 11.1 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 9.9 mm²/s Show Material materials with Difusividad térmica of 9.9 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 8.7 mm²/s Show Material materials with Difusividad térmica of 8.7 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 7.3 mm²/s Show Material materials with Difusividad térmica of 7.3 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 20 - 400 °C Show Material materials with Temperatura máx. de funcionamiento of 20 - 400 °C | normalized or normalized formed (+N) | EN 10028-2 | Flat | Long | |
400 °C Show Material materials with Temperatura máx. de funcionamiento of 400 °C | normalized or normalized formed (+N) | EN 10028-2 | Flat | Long | ||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 6 S/m Show Material materials with Conductividad eléctrica of 6 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 2.2e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 2.2e-07 - 2.24e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.2e-07 - 2.24e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 2.24e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.24e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 2.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.7e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 2.7e-07 - 2.71e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.7e-07 - 2.71e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 2.71e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.71e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.4e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.4e-07 - 3.44e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-07 - 3.44e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.44e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.44e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.3e-07 - 4.31e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-07 - 4.31e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.31e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.31e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.3e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.3e-07 - 5.32e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.3e-07 - 5.32e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.32e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.32e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.5e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.5e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.86e-07 - 7.9e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.86e-07 - 7.9e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.86e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.86e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.9e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.9e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
0.015 % Show Material materials with Azufre of 0.015 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
Carbono | 0.08 - 0.2 % Show Material materials with Carbono of 0.08 - 0.2 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Manganeso | 0.9 - 1.5 % Show Material materials with Manganeso of 0.9 - 1.5 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Molibdeno | 0.08 % Show Material materials with Molibdeno of 0.08 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Niobio | 0.02 % Show Material materials with Niobio of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Níquel | 0.3 % Show Material materials with Níquel of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Vanadio | 0.02 % Show Material materials with Vanadio of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |