General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.82 g/cm³ Show Material materials with Densidad of 7.82 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
20 °C | 7.82 - 7.83 g/cm³ Show Material materials with Densidad of 7.82 - 7.83 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel | ||||
Dureza Brinell | 245 [-] Show Material materials with Dureza Brinell of 245 [-] | Predicted Value, Transverse | ||||
Elongación | 15.2 % Show Material materials with Elongación of 15.2 % | Predicted Value, A80 Transverse | ||||
15.4 % Show Material materials with Elongación of 15.4 % | Predicted Value, A80 | |||||
15.4 % Show Material materials with Elongación of 15.4 % | Predicted Value, A200 | |||||
16.7 % Show Material materials with Elongación of 16.7 % | Predicted Value, A5 | |||||
19.1 % Show Material materials with Elongación of 19.1 % | Predicted Value, A50 | |||||
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Estricción | 38.7 % Show Material materials with Estricción of 38.7 % | Predicted Value | ||||
44.2 % Show Material materials with Estricción of 44.2 % | Predicted Value, Transverse | |||||
Límite elástico | 289.3 MPa Show Material materials with Límite elástico of 289.3 MPa | Predicted Value, RP1 Transverse | ||||
297.5 MPa Show Material materials with Límite elástico of 297.5 MPa | Predicted Value, RP1 | |||||
432 MPa Show Material materials with Límite elástico of 432 MPa | Predicted Value, RP05 | |||||
451.1 MPa Show Material materials with Límite elástico of 451.1 MPa | Predicted Value, RP02 Transverse | |||||
601.7 MPa Show Material materials with Límite elástico of 601.7 MPa | Predicted Value, RP002 | |||||
20 °C | 280 MPa Show Material materials with Límite elástico of 280 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 280 MPa Show Material materials with Límite elástico of 280 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 315 MPa Show Material materials with Límite elástico of 315 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 315 MPa Show Material materials with Límite elástico of 315 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 335 MPa Show Material materials with Límite elástico of 335 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 335 MPa Show Material materials with Límite elástico of 335 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
50 °C | 271 MPa Show Material materials with Límite elástico of 271 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 305 MPa Show Material materials with Límite elástico of 305 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 324 MPa Show Material materials with Límite elástico of 324 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 334 MPa Show Material materials with Límite elástico of 334 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 343 MPa Show Material materials with Límite elástico of 343 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 255 MPa Show Material materials with Límite elástico of 255 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 268 MPa Show Material materials with Límite elástico of 268 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 287 MPa Show Material materials with Límite elástico of 287 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 305 MPa Show Material materials with Límite elástico of 305 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 314 MPa Show Material materials with Límite elástico of 314 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 323 MPa Show Material materials with Límite elástico of 323 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 236 MPa Show Material materials with Límite elástico of 236 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 249 MPa Show Material materials with Límite elástico of 249 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 265 MPa Show Material materials with Límite elástico of 265 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 282 MPa Show Material materials with Límite elástico of 282 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 291 MPa Show Material materials with Límite elástico of 291 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 299 MPa Show Material materials with Límite elástico of 299 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 217 MPa Show Material materials with Límite elástico of 217 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 228 MPa Show Material materials with Límite elástico of 228 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 244 MPa Show Material materials with Límite elástico of 244 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 259 MPa Show Material materials with Límite elástico of 259 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 267 MPa Show Material materials with Límite elástico of 267 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 199 MPa Show Material materials with Límite elástico of 199 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 209 MPa Show Material materials with Límite elástico of 209 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 224 MPa Show Material materials with Límite elástico of 224 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 238 MPa Show Material materials with Límite elástico of 238 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 245 MPa Show Material materials with Límite elástico of 245 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 252 MPa Show Material materials with Límite elástico of 252 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 183 MPa Show Material materials with Límite elástico of 183 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 192 MPa Show Material materials with Límite elástico of 192 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 206 MPa Show Material materials with Límite elástico of 206 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 219 MPa Show Material materials with Límite elástico of 219 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 232 MPa Show Material materials with Límite elástico of 232 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 169 MPa Show Material materials with Límite elástico of 169 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 178 MPa Show Material materials with Límite elástico of 178 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 190 MPa Show Material materials with Límite elástico of 190 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 202 MPa Show Material materials with Límite elástico of 202 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 208 MPa Show Material materials with Límite elástico of 208 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 214 MPa Show Material materials with Límite elástico of 214 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 159 MPa Show Material materials with Límite elástico of 159 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 167 MPa Show Material materials with Límite elástico of 167 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 179 MPa Show Material materials with Límite elástico of 179 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 190 MPa Show Material materials with Límite elástico of 190 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 196 MPa Show Material materials with Límite elástico of 196 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 202 MPa Show Material materials with Límite elástico of 202 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 207 - 208 GPa Show Material materials with Módulo elástico of 207 - 208 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 208 GPa Show Material materials with Módulo elástico of 208 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 199 - 201 GPa Show Material materials with Módulo elástico of 199 - 201 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 201 GPa Show Material materials with Módulo elástico of 201 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 192 - 193 GPa Show Material materials with Módulo elástico of 192 - 193 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 193 GPa Show Material materials with Módulo elástico of 193 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 184 - 185 GPa Show Material materials with Módulo elástico of 184 - 185 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 185 GPa Show Material materials with Módulo elástico of 185 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Resistencia a la tracción | 20 °C | 470 - 650 MPa Show Material materials with Resistencia a la tracción of 470 - 650 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse |
20 °C | 470 - 630 MPa Show Material materials with Resistencia a la tracción of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 470 - 650 MPa Show Material materials with Resistencia a la tracción of 470 - 650 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 470 - 630 MPa Show Material materials with Resistencia a la tracción of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 480 - 650 MPa Show Material materials with Resistencia a la tracción of 480 - 650 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 480 - 630 MPa Show Material materials with Resistencia a la tracción of 480 - 630 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 480 - 650 MPa Show Material materials with Resistencia a la tracción of 480 - 650 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 480 - 630 MPa Show Material materials with Resistencia a la tracción of 480 - 630 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 490 - 650 MPa Show Material materials with Resistencia a la tracción of 490 - 650 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 490 - 630 MPa Show Material materials with Resistencia a la tracción of 490 - 630 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 490 - 650 MPa Show Material materials with Resistencia a la tracción of 490 - 650 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 490 - 630 MPa Show Material materials with Resistencia a la tracción of 490 - 630 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 510 - 650 MPa Show Material materials with Resistencia a la tracción of 510 - 650 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 510 - 630 MPa Show Material materials with Resistencia a la tracción of 510 - 630 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 510 - 650 MPa Show Material materials with Resistencia a la tracción of 510 - 650 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 510 - 630 MPa Show Material materials with Resistencia a la tracción of 510 - 630 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Resistencia al cizallamiento | 550.7 MPa Show Material materials with Resistencia al cizallamiento of 550.7 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Calor específico of 430 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Calor específico of 430 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Calor específico of 479 - 500 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Calor específico of 499 - 540 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 540 J/(kg·K) Show Material materials with Calor específico of 540 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 517 - 580 J/(kg·K) Show Material materials with Calor específico of 517 - 580 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 580 J/(kg·K) Show Material materials with Calor específico of 580 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Calor específico of 536 - 620 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 620 J/(kg·K) Show Material materials with Calor específico of 620 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 558 - 690 J/(kg·K) Show Material materials with Calor específico of 558 - 690 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 690 J/(kg·K) Show Material materials with Calor específico of 690 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 587 - 780 J/(kg·K) Show Material materials with Calor específico of 587 - 780 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 780 J/(kg·K) Show Material materials with Calor específico of 780 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 1.22e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 1.22e-05 - 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22e-05 - 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.29e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.29e-05 - 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29e-05 - 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.34e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.34e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.34e-05 - 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.34e-05 - 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.4e-05 - 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 - 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.43e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 - 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.43e-05 - 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.46e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.46e-05 - 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.46e-05 - 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Conductividad térmica | 20 °C | 39.7 - 40 W/(m·K) Show Material materials with Conductividad térmica of 39.7 - 40 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 39.7 W/(m·K) Show Material materials with Conductividad térmica of 39.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 40 W/(m·K) Show Material materials with Conductividad térmica of 40 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 41 W/(m·K) Show Material materials with Conductividad térmica of 41 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 41 - 41.3 W/(m·K) Show Material materials with Conductividad térmica of 41 - 41.3 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 41.3 W/(m·K) Show Material materials with Conductividad térmica of 41.3 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 41 W/(m·K) Show Material materials with Conductividad térmica of 41 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 41 - 41.5 W/(m·K) Show Material materials with Conductividad térmica of 41 - 41.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 41.5 W/(m·K) Show Material materials with Conductividad térmica of 41.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 40 W/(m·K) Show Material materials with Conductividad térmica of 40 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 40 - 40.4 W/(m·K) Show Material materials with Conductividad térmica of 40 - 40.4 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 40.4 W/(m·K) Show Material materials with Conductividad térmica of 40.4 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 38 W/(m·K) Show Material materials with Conductividad térmica of 38 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 38 - 38.7 W/(m·K) Show Material materials with Conductividad térmica of 38 - 38.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 38.7 W/(m·K) Show Material materials with Conductividad térmica of 38.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 36 W/(m·K) Show Material materials with Conductividad térmica of 36 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 36 - 36.6 W/(m·K) Show Material materials with Conductividad térmica of 36 - 36.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 36.6 W/(m·K) Show Material materials with Conductividad térmica of 36.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 34 W/(m·K) Show Material materials with Conductividad térmica of 34 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 34 - 34.3 W/(m·K) Show Material materials with Conductividad térmica of 34 - 34.3 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 34.3 W/(m·K) Show Material materials with Conductividad térmica of 34.3 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Difusividad térmica | 20 °C | 11 mm²/s Show Material materials with Difusividad térmica of 11 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
100 °C | 10.7 mm²/s Show Material materials with Difusividad térmica of 10.7 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 10 mm²/s Show Material materials with Difusividad térmica of 10 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 8.2 mm²/s Show Material materials with Difusividad térmica of 8.2 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 7.1 mm²/s Show Material materials with Difusividad térmica of 7.1 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 5.8 mm²/s Show Material materials with Difusividad térmica of 5.8 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 20 - 400 °C Show Material materials with Temperatura máx. de funcionamiento of 20 - 400 °C | normalized or normalized formed (+N) | EN 10028-2 | Flat | Long | |
400 °C Show Material materials with Temperatura máx. de funcionamiento of 400 °C | normalized or normalized formed (+N) | EN 10028-2 | Flat | Long | ||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 6 S/m Show Material materials with Conductividad eléctrica of 6 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 2.6e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.6e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 2.6e-07 - 2.62e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.6e-07 - 2.62e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 2.62e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.62e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 3.1e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.1e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.8e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.64e-07 - 4.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.64e-07 - 4.7e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.64e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.64e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.62e-07 - 5.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.62e-07 - 5.7e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.62e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.62e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.7e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.76e-07 - 6.9e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.76e-07 - 6.9e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.76e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.76e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.9e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.9e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 8.07e-07 - 8.2e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.07e-07 - 8.2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 8.07e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.07e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 8.2e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
0.015 % Show Material materials with Azufre of 0.015 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
Carbono | 0.1 - 0.22 % Show Material materials with Carbono of 0.1 - 0.22 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Manganeso | 1.1 - 1.7 % Show Material materials with Manganeso of 1.1 - 1.7 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Molibdeno | 0.08 % Show Material materials with Molibdeno of 0.08 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Niobio | 0.02 % Show Material materials with Niobio of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
0.04 % Show Material materials with Niobio of 0.04 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Níquel | 0.3 % Show Material materials with Níquel of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Vanadio | 0.02 % Show Material materials with Vanadio of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Technological properties
Property | ||
---|---|---|