General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.83 - 7.84 g/cm³ Show Material materials with Densidad of 7.83 - 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat |
20 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel | ||||
Dureza Brinell | 240 [-] Show Material materials with Dureza Brinell of 240 [-] | Predicted Value, Transverse | ||||
Elongación | 16.9 % Show Material materials with Elongación of 16.9 % | Predicted Value, A80 Transverse | ||||
17.2 % Show Material materials with Elongación of 17.2 % | Predicted Value, A80 | |||||
17.8 % Show Material materials with Elongación of 17.8 % | Predicted Value, A200 | |||||
20.3 % Show Material materials with Elongación of 20.3 % | Predicted Value, Transverse | |||||
20.6 % Show Material materials with Elongación of 20.6 % | Predicted Value, A50 | |||||
21.2 % Show Material materials with Elongación of 21.2 % | Predicted Value, A5 | |||||
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Estricción | 39.1 % Show Material materials with Estricción of 39.1 % | Predicted Value | ||||
43.9 % Show Material materials with Estricción of 43.9 % | Predicted Value, Transverse | |||||
Límite elástico | 260.2 MPa Show Material materials with Límite elástico of 260.2 MPa | Predicted Value, RP1 | ||||
315.1 MPa Show Material materials with Límite elástico of 315.1 MPa | Predicted Value, RP1 Transverse | |||||
365.8 MPa Show Material materials with Límite elástico of 365.8 MPa | Predicted Value, Transverse | |||||
458.1 MPa Show Material materials with Límite elástico of 458.1 MPa | Predicted Value, RP02 Transverse | |||||
460.4 MPa Show Material materials with Límite elástico of 460.4 MPa | Predicted Value, RP05 | |||||
464 MPa Show Material materials with Límite elástico of 464 MPa | Predicted Value, RP002 | |||||
20 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 305 MPa Show Material materials with Límite elástico of 305 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 315 MPa Show Material materials with Límite elástico of 315 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 335 MPa Show Material materials with Límite elástico of 335 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
50 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
50 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 305 MPa Show Material materials with Límite elástico of 305 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 324 MPa Show Material materials with Límite elástico of 324 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 334 MPa Show Material materials with Límite elástico of 334 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 343 MPa Show Material materials with Límite elástico of 343 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 245 MPa Show Material materials with Límite elástico of 245 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
100 °C | 268 MPa Show Material materials with Límite elástico of 268 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 277 MPa Show Material materials with Límite elástico of 277 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 287 MPa Show Material materials with Límite elástico of 287 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 305 MPa Show Material materials with Límite elástico of 305 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 314 MPa Show Material materials with Límite elástico of 314 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 323 MPa Show Material materials with Límite elástico of 323 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
150 °C | 249 MPa Show Material materials with Límite elástico of 249 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 257 MPa Show Material materials with Límite elástico of 257 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 265 MPa Show Material materials with Límite elástico of 265 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 282 MPa Show Material materials with Límite elástico of 282 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 291 MPa Show Material materials with Límite elástico of 291 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 299 MPa Show Material materials with Límite elástico of 299 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 206 MPa Show Material materials with Límite elástico of 206 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
200 °C | 228 MPa Show Material materials with Límite elástico of 228 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 236 MPa Show Material materials with Límite elástico of 236 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 244 MPa Show Material materials with Límite elástico of 244 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 259 MPa Show Material materials with Límite elástico of 259 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 267 MPa Show Material materials with Límite elástico of 267 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
250 °C | 186 MPa Show Material materials with Límite elástico of 186 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
250 °C | 209 MPa Show Material materials with Límite elástico of 209 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 216 MPa Show Material materials with Límite elástico of 216 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 224 MPa Show Material materials with Límite elástico of 224 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 238 MPa Show Material materials with Límite elástico of 238 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 245 MPa Show Material materials with Límite elástico of 245 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
250 °C | 252 MPa Show Material materials with Límite elástico of 252 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 167 MPa Show Material materials with Límite elástico of 167 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
300 °C | 192 MPa Show Material materials with Límite elástico of 192 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 199 MPa Show Material materials with Límite elástico of 199 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 206 MPa Show Material materials with Límite elástico of 206 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
300 °C | 219 MPa Show Material materials with Límite elástico of 219 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
300 °C | 232 MPa Show Material materials with Límite elástico of 232 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 147 MPa Show Material materials with Límite elástico of 147 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
350 °C | 178 MPa Show Material materials with Límite elástico of 178 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 184 MPa Show Material materials with Límite elástico of 184 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 190 MPa Show Material materials with Límite elástico of 190 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 202 MPa Show Material materials with Límite elástico of 202 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 208 MPa Show Material materials with Límite elástico of 208 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 214 MPa Show Material materials with Límite elástico of 214 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 117 MPa Show Material materials with Límite elástico of 117 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
400 °C | 167 MPa Show Material materials with Límite elástico of 167 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
400 °C | 173 MPa Show Material materials with Límite elástico of 173 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 179 MPa Show Material materials with Límite elástico of 179 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 190 MPa Show Material materials with Límite elástico of 190 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 196 MPa Show Material materials with Límite elástico of 196 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 202 MPa Show Material materials with Límite elástico of 202 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Resistencia a la tracción | 20 °C | 440 - 590 MPa Show Material materials with Resistencia a la tracción of 440 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | |
20 °C | 450 - 630 MPa Show Material materials with Resistencia a la tracción of 450 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 450 - 610 MPa Show Material materials with Resistencia a la tracción of 450 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 450 - 600 MPa Show Material materials with Resistencia a la tracción of 450 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 450 - 590 MPa Show Material materials with Resistencia a la tracción of 450 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 630 MPa Show Material materials with Resistencia a la tracción of 460 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 610 MPa Show Material materials with Resistencia a la tracción of 460 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 600 MPa Show Material materials with Resistencia a la tracción of 460 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 590 MPa Show Material materials with Resistencia a la tracción of 460 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 630 MPa Show Material materials with Resistencia a la tracción of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 610 MPa Show Material materials with Resistencia a la tracción of 470 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 600 MPa Show Material materials with Resistencia a la tracción of 470 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 590 MPa Show Material materials with Resistencia a la tracción of 470 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 630 MPa Show Material materials with Resistencia a la tracción of 490 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 610 MPa Show Material materials with Resistencia a la tracción of 490 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 600 MPa Show Material materials with Resistencia a la tracción of 490 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 590 MPa Show Material materials with Resistencia a la tracción of 490 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Resistencia al cizallamiento | 516.8 MPa Show Material materials with Resistencia al cizallamiento of 516.8 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Calor específico of 430 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Calor específico of 430 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Conductividad térmica | -100 °C | 37.6 W/(m·K) Show Material materials with Conductividad térmica of 37.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 42 W/(m·K) Show Material materials with Conductividad térmica of 42 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 42 - 42.2 W/(m·K) Show Material materials with Conductividad térmica of 42 - 42.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 42.2 W/(m·K) Show Material materials with Conductividad térmica of 42.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 43.2 W/(m·K) Show Material materials with Conductividad térmica of 43.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 42.9 W/(m·K) Show Material materials with Conductividad térmica of 42.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 41.2 W/(m·K) Show Material materials with Conductividad térmica of 41.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 39.1 W/(m·K) Show Material materials with Conductividad térmica of 39.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 36.6 W/(m·K) Show Material materials with Conductividad térmica of 36.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 34.1 W/(m·K) Show Material materials with Conductividad térmica of 34.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Difusividad térmica | -100 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 11.7 mm²/s Show Material materials with Difusividad térmica of 11.7 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 11.2 mm²/s Show Material materials with Difusividad térmica of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 10.3 mm²/s Show Material materials with Difusividad térmica of 10.3 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 9.4 mm²/s Show Material materials with Difusividad térmica of 9.4 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 8.3 mm²/s Show Material materials with Difusividad térmica of 8.3 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 7.1 mm²/s Show Material materials with Difusividad térmica of 7.1 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | -20 - 400 °C Show Material materials with Temperatura máx. de funcionamiento of -20 - 400 °C | normalized or normalized formed (+N) | EN 10028-3 | Flat | Long | |
400 °C Show Material materials with Temperatura máx. de funcionamiento of 400 °C | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | Long | ||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 5 S/m Show Material materials with Conductividad eléctrica of 5 S/m | Predicted Value | ||||
Resistividad eléctrica | -100 °C | 1.82e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.82e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 2.47e-07 - 2.5e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.47e-07 - 2.5e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.47e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.47e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.5e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.5e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 2.96e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.96e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 3.68e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.68e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 4.55e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.55e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 5.56e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.56e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 6.75e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.75e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 8.13e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.13e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Carbono | 0.18 % Show Material materials with Carbono of 0.18 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Manganeso | 1.1 - 1.7 % Show Material materials with Manganeso of 1.1 - 1.7 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Molibdeno | 0.08 % Show Material materials with Molibdeno of 0.08 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Niobio | 0.05 % Show Material materials with Niobio of 0.05 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Níquel | 0.5 % Show Material materials with Níquel of 0.5 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Vanadio | 0.1 % Show Material materials with Vanadio of 0.1 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |