General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10028-4 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.291 [-] Show Material materials with Coeficiente de Poisson of 0.291 [-] | Typical for Nickel Steel | ||||
Elongación | 16.9 % Show Material materials with Elongación of 16.9 % | Predicted Value, A80 | ||||
17.7 % Show Material materials with Elongación of 17.7 % | Predicted Value, A200 | |||||
17.9 % Show Material materials with Elongación of 17.9 % | Predicted Value, A80 Transverse | |||||
20.4 % Show Material materials with Elongación of 20.4 % | Predicted Value, A50 | |||||
20.4 % Show Material materials with Elongación of 20.4 % | Predicted Value, Transverse | |||||
22.5 % Show Material materials with Elongación of 22.5 % | Predicted Value, A5 | |||||
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
Estricción | 43.2 % Show Material materials with Estricción of 43.2 % | Predicted Value, Transverse | ||||
43.9 % Show Material materials with Estricción of 43.9 % | Predicted Value | |||||
Límite elástico | 259.6 MPa Show Material materials with Límite elástico of 259.6 MPa | Predicted Value, RP1 | ||||
315.6 MPa Show Material materials with Límite elástico of 315.6 MPa | Predicted Value, RP1 Transverse | |||||
367.5 MPa Show Material materials with Límite elástico of 367.5 MPa | Predicted Value, Transverse | |||||
373.6 MPa Show Material materials with Límite elástico of 373.6 MPa | Predicted Value, RP05 | |||||
386.6 MPa Show Material materials with Límite elástico of 386.6 MPa | Predicted Value, RP02 | |||||
460.3 MPa Show Material materials with Límite elástico of 460.3 MPa | Predicted Value, RP002 | |||||
481.2 MPa Show Material materials with Límite elástico of 481.2 MPa | Predicted Value, RP02 Transverse | |||||
20 °C | 335 MPa Show Material materials with Límite elástico of 335 MPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
20 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
Módulo de cizallamiento | 76 GPa Show Material materials with Módulo de cizallamiento of 76 GPa | Typical for Nickel Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
Resistencia a la tracción | 20 °C | 490 - 640 MPa Show Material materials with Resistencia a la tracción of 490 - 640 MPa | normalized or normalized formed (+N) | EN 10028-4 | Flat | |
Resistencia al cizallamiento | 551.8 MPa Show Material materials with Resistencia al cizallamiento of 551.8 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.05e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05e-05 1/K | normalized or normalized formed (+N) | EN 10028-4 | Flat | |
20 °C | 1.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15e-05 1/K | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21e-05 1/K | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27e-05 1/K | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 1/K | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44e-05 1/K | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
Conductividad térmica | 20 °C | 42.5 W/(m·K) Show Material materials with Conductividad térmica of 42.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | |
100 °C | 43.5 W/(m·K) Show Material materials with Conductividad térmica of 43.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
200 °C | 42.8 W/(m·K) Show Material materials with Conductividad térmica of 42.8 W/(m·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
300 °C | 40.9 W/(m·K) Show Material materials with Conductividad térmica of 40.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
400 °C | 39 W/(m·K) Show Material materials with Conductividad térmica of 39 W/(m·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
500 °C | 36.4 W/(m·K) Show Material materials with Conductividad térmica of 36.4 W/(m·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
600 °C | 34.1 W/(m·K) Show Material materials with Conductividad térmica of 34.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
Difusividad térmica | 20 °C | 11.7 mm²/s Show Material materials with Difusividad térmica of 11.7 mm²/s | normalized or normalized formed (+N) | EN 10028-4 | Flat | |
100 °C | 11.2 mm²/s Show Material materials with Difusividad térmica of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
200 °C | 10.3 mm²/s Show Material materials with Difusividad térmica of 10.3 mm²/s | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
300 °C | 9.3 mm²/s Show Material materials with Difusividad térmica of 9.3 mm²/s | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
400 °C | 8.3 mm²/s Show Material materials with Difusividad térmica of 8.3 mm²/s | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
500 °C | 7 mm²/s Show Material materials with Difusividad térmica of 7 mm²/s | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
Temperatura de fusión | 1316 - 1595 °C Show Material materials with Temperatura de fusión of 1316 - 1595 °C | Typical for Nickel Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 7 S/m Show Material materials with Conductividad eléctrica of 7 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 2.45e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.45e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-4 | Flat | |
100 °C | 2.94e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.94e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
200 °C | 3.69e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.69e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
300 °C | 4.59e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.59e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
400 °C | 5.58e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.58e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
500 °C | 6.79e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.79e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-4 | Flat | ||
600 °C | 8.13e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.13e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-4 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | normalized or normalized formed (+N) | EN 10028-4 | Flat |
0.015 % Show Material materials with Azufre of 0.015 % | normalized or normalized formed (+N) | EN 10028-4 | Flat | |
Carbono | 0.18 % Show Material materials with Carbono of 0.18 % | normalized or normalized formed (+N) | EN 10028-4 | Flat |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10028-4 | Flat |
Manganeso | 0.8 - 1.5 % Show Material materials with Manganeso of 0.8 - 1.5 % | normalized or normalized formed (+N) | EN 10028-4 | Flat |
Níquel | 1.3 - 1.7 % Show Material materials with Níquel of 1.3 - 1.7 % | normalized or normalized formed (+N) | EN 10028-4 | Flat |
Silicona | 0.35 % Show Material materials with Silicona of 0.35 % | normalized or normalized formed (+N) | EN 10028-4 | Flat |
Vanadio | 0.05 % Show Material materials with Vanadio of 0.05 % | normalized or normalized formed (+N) | EN 10028-4 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |