General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel | ||||
Dureza Brinell | 243 [-] Show Material materials with Dureza Brinell of 243 [-] | Predicted Value, Transverse | ||||
Elongación | 17.0 % Show Material materials with Elongación of 17.0 % | Predicted Value, A80 Transverse | ||||
17.3 % Show Material materials with Elongación of 17.3 % | Predicted Value, A80 | |||||
17.9 % Show Material materials with Elongación of 17.9 % | Predicted Value, A200 | |||||
19.6 % Show Material materials with Elongación of 19.6 % | Predicted Value, Transverse | |||||
21.1 % Show Material materials with Elongación of 21.1 % | Predicted Value, A5 | |||||
21.4 % Show Material materials with Elongación of 21.4 % | Predicted Value, A50 | |||||
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat | ||
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
Estricción | 43.8 % Show Material materials with Estricción of 43.8 % | Predicted Value, Transverse | ||||
52.2 % Show Material materials with Estricción of 52.2 % | Predicted Value | |||||
Límite elástico | 254.1 MPa Show Material materials with Límite elástico of 254.1 MPa | Predicted Value, RP1 | ||||
301.2 MPa Show Material materials with Límite elástico of 301.2 MPa | Predicted Value, RP1 Transverse | |||||
360.3 MPa Show Material materials with Límite elástico of 360.3 MPa | Predicted Value, RP02 | |||||
376.2 MPa Show Material materials with Límite elástico of 376.2 MPa | Predicted Value, Transverse | |||||
453.9 MPa Show Material materials with Límite elástico of 453.9 MPa | Predicted Value, RP02 Transverse | |||||
462.2 MPa Show Material materials with Límite elástico of 462.2 MPa | Predicted Value, RP002 | |||||
465.6 MPa Show Material materials with Límite elástico of 465.6 MPa | Predicted Value, RP05 | |||||
20 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat, Strip, Rod, Wire | ||
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 315 MPa Show Material materials with Límite elástico of 315 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 325 MPa Show Material materials with Límite elástico of 325 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 335 MPa Show Material materials with Límite elástico of 335 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Resistencia a la tracción | 20 °C | 440 - 590 MPa Show Material materials with Resistencia a la tracción of 440 - 590 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat | |
20 °C | 450 - 630 MPa Show Material materials with Resistencia a la tracción of 450 - 630 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 450 - 600 MPa Show Material materials with Resistencia a la tracción of 450 - 600 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 470 - 630 MPa Show Material materials with Resistencia a la tracción of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 470 - 600 MPa Show Material materials with Resistencia a la tracción of 470 - 600 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
Resistencia al cizallamiento | 513.5 MPa Show Material materials with Resistencia al cizallamiento of 513.5 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Conductividad térmica | -100 °C | 37.6 W/(m·K) Show Material materials with Conductividad térmica of 37.6 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 42.2 W/(m·K) Show Material materials with Conductividad térmica of 42.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 43.2 W/(m·K) Show Material materials with Conductividad térmica of 43.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 42.9 W/(m·K) Show Material materials with Conductividad térmica of 42.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 41.2 W/(m·K) Show Material materials with Conductividad térmica of 41.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 39.1 W/(m·K) Show Material materials with Conductividad térmica of 39.1 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 36.6 W/(m·K) Show Material materials with Conductividad térmica of 36.6 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 34.1 W/(m·K) Show Material materials with Conductividad térmica of 34.1 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Difusividad térmica | -100 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 11.7 mm²/s Show Material materials with Difusividad térmica of 11.7 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 11.2 mm²/s Show Material materials with Difusividad térmica of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 10.3 mm²/s Show Material materials with Difusividad térmica of 10.3 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 9.4 mm²/s Show Material materials with Difusividad térmica of 9.4 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 8.3 mm²/s Show Material materials with Difusividad térmica of 8.3 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 7.1 mm²/s Show Material materials with Difusividad térmica of 7.1 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 368.7 °C Show Material materials with Temperatura máx. de funcionamiento of 368.7 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 5 S/m Show Material materials with Conductividad eléctrica of 5 S/m | Predicted Value | ||||
Resistividad eléctrica | -100 °C | 1.82e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.82e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 2.47e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.47e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 2.96e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.96e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 3.68e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.68e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 4.55e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.55e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 5.56e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.56e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 6.75e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.75e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 8.13e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.13e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Azufre | 0.02 % Show Material materials with Azufre of 0.02 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.025 % Show Material materials with Azufre of 0.025 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Carbono | 0.18 % Show Material materials with Carbono of 0.18 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Cobre | 0.35 % Show Material materials with Cobre of 0.35 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.55 % Show Material materials with Cobre of 0.55 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.03 % Show Material materials with Fósforo of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Manganeso | 0.9 - 1.65 % Show Material materials with Manganeso of 0.9 - 1.65 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Molibdeno | 0.1 % Show Material materials with Molibdeno of 0.1 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Niobio | 0.05 % Show Material materials with Niobio of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Nitrógeno | 0.015 % Show Material materials with Nitrógeno of 0.015 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Níquel | 0.5 % Show Material materials with Níquel of 0.5 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.05 % Show Material materials with Titanio of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Vanadio | 0.12 % Show Material materials with Vanadio of 0.12 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Technological properties
Property | ||
---|---|---|