General
Property | Value | Comment |
---|---|---|
Densidad | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | Typical for Steel |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel | ||||
Elongación | 17.4 % Show Material materials with Elongación of 17.4 % | Predicted Value, A200 | ||||
21.8 % Show Material materials with Elongación of 21.8 % | Predicted Value, A5 | |||||
23.1 % Show Material materials with Elongación of 23.1 % | Predicted Value, A50 | |||||
20 °C | 14 % Show Material materials with Elongación of 14 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire | ||
Límite elástico | 261 MPa Show Material materials with Límite elástico of 261 MPa | Predicted Value, RP1 | ||||
286.6 MPa Show Material materials with Límite elástico of 286.6 MPa | Predicted Value, RP1 Transverse | |||||
390 MPa Show Material materials with Límite elástico of 390 MPa | Predicted Value, RP02 | |||||
401.5 MPa Show Material materials with Límite elástico of 401.5 MPa | Predicted Value, RP05 | |||||
406.7 MPa Show Material materials with Límite elástico of 406.7 MPa | Predicted Value, RP02 Transverse | |||||
468.6 MPa Show Material materials with Límite elástico of 468.6 MPa | Predicted Value, RP002 | |||||
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 315 MPa Show Material materials with Límite elástico of 315 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 315 MPa Show Material materials with Límite elástico of 315 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 325 MPa Show Material materials with Límite elástico of 325 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 325 MPa Show Material materials with Límite elástico of 325 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 335 MPa Show Material materials with Límite elástico of 335 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 335 MPa Show Material materials with Límite elástico of 335 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Módulo elástico | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel | ||||
Resistencia a la tracción | 20 °C | 450 - 680 MPa Show Material materials with Resistencia a la tracción of 450 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse |
20 °C | 450 - 630 MPa Show Material materials with Resistencia a la tracción of 450 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 450 - 600 MPa Show Material materials with Resistencia a la tracción of 450 - 600 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 450 - 680 MPa Show Material materials with Resistencia a la tracción of 450 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 450 - 630 MPa Show Material materials with Resistencia a la tracción of 450 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 450 - 600 MPa Show Material materials with Resistencia a la tracción of 450 - 600 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 680 MPa Show Material materials with Resistencia a la tracción of 470 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 470 - 630 MPa Show Material materials with Resistencia a la tracción of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 470 - 600 MPa Show Material materials with Resistencia a la tracción of 470 - 600 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 470 - 680 MPa Show Material materials with Resistencia a la tracción of 470 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 630 MPa Show Material materials with Resistencia a la tracción of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 600 MPa Show Material materials with Resistencia a la tracción of 470 - 600 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 490 - 680 MPa Show Material materials with Resistencia a la tracción of 490 - 680 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | ||
20 °C | 490 - 630 MPa Show Material materials with Resistencia a la tracción of 490 - 630 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | ||
20 °C | 510 - 680 MPa Show Material materials with Resistencia a la tracción of 510 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 510 - 630 MPa Show Material materials with Resistencia a la tracción of 510 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 510 - 600 MPa Show Material materials with Resistencia a la tracción of 510 - 600 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 510 - 680 MPa Show Material materials with Resistencia a la tracción of 510 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 510 - 630 MPa Show Material materials with Resistencia a la tracción of 510 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 510 - 600 MPa Show Material materials with Resistencia a la tracción of 510 - 600 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire |
0.04 % Show Material materials with Azufre of 0.04 % | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
Carbono | 0.16 % Show Material materials with Carbono of 0.16 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Circonio | 0.15 % Show Material materials with Circonio of 0.15 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Cobre | 0.25 - 0.55 % Show Material materials with Cobre of 0.25 - 0.55 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Cromo | 0.4 - 0.8 % Show Material materials with Cromo of 0.4 - 0.8 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Fósforo | 0.035 % Show Material materials with Fósforo of 0.035 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire |
0.04 % Show Material materials with Fósforo of 0.04 % | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
Manganeso | 0.5 - 1.5 % Show Material materials with Manganeso of 0.5 - 1.5 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire |
0.5 - 1 % Show Material materials with Manganeso of 0.5 - 1 % | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
Molibdeno | 0.3 % Show Material materials with Molibdeno of 0.3 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Nitrógeno | 0.009 % Show Material materials with Nitrógeno of 0.009 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Níquel | 0.65 % Show Material materials with Níquel of 0.65 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |